  1. 1Types and manufacture
  2. 2Fire behaviour compared with solid wood
  3. 3Ignition and self-heating
  4. 4Flame spread and heat release
  5. 5Fire resistance and charring
  6. 6Fire-retardant treatment
  7. 7Regulation and classification
  8. 8See also
  9. 9Notes
  10. 10References

Wood-based panel products are flat boards made by bonding wood veneers, strands, flakes, particles or fibres together with an adhesive resin under heat and pressure. The family includes plywood, oriented strand board (OSB), particleboard (also called chipboard), medium-density fibreboard (MDF), hardboard and insulation board.[1][2] The NFPA Fire Protection Handbook calls them secondary forest products, because processing beyond cutting and drying is needed to make them.[3] Panels burn in the same basic way as the wood they are made from. Their low moisture content, thin sections and resin binders, however, make many of them easier to ignite and quicker to spread flame than solid timber.[4][5]

In the United States tunnel test, untreated plywood and particleboard reach flame spread indices of about 95 to 200, and old low-density fibreboard ceilings have rated much worse.[6][7] Their contribution to the fire resistance of a wall or floor grows with thickness and density.[8] Fire-retardant treatment can bring the flame spread index of a panel down to 25 or less, but no treatment makes it noncombustible.[6][9]

Types and manufacture

The handbook groups wood products by the amount of processing they need. Primary forest products, such as structural timbers, dimension lumber, shingles and veneers, need only cutting and drying. Products such as plywood, flakeboard, strandboard, particleboard, fibreboard, insulation board and ceiling tile need further processes and are therefore secondary forest products.[3] Shaw (2008) uses the term wood-based composite panels for boards of fibres, particles or flakes mixed with a binder and formed under pressure. They keep some properties of the original wood, but the manufacturing method gives them new and different ones.[1]

Two construction principles are used. Plywood and laminated veneer lumber are built from thin sheets of wood, called veneer, glued together, which overcomes the dimensional instability of sawn lumber.[4] Softwood plies range from about 1.1 mm for face plies to 3.2 mm for core plies.[10] In the other panel types the log is reduced to flakes, strands, splinters, fibres or particles, which are mixed with thermoset plastic resins and pressed into a composite.[2] This also reduces waste: in producing traditional dimension lumber almost 25 percent of the wood in the tree ends up as waste, and another 25 percent before the finished product.[10]

Four panel cross-sections: plywood with crossed veneers, OSB with large strands, particleboard with fine particles, MDF with fibres.
The main wood-based panel types: plywood from glued veneers, and OSB, particleboard and fibreboard from strands, particles or fibres bonded with a thermoset resin.

In a particleboard plant the particulate is screened and dried, usually to below 7 percent moisture, often in rotary drum dryers.[11][12] It is blended with a thermoset adhesive resin and laid on a steel belt as a layered mat, which a gang press or a continuous press compresses at high pressure and temperature.[13] The presses are often heated with heat transfer fluid, a thermal oil that can escape as an atomised spray above its flash point if a line leaks. These hazards, together with dryers and dust, are treated under Woodworking facility.[13] The International Fire Engineering Guidelines (2005) list fire load densities of 800 MJ/m² for chipboard finishing and for plywood manufacture, and 100 MJ/m² for chipboard pressing.[14]

Panels form a large share of the wood used in the United States and abroad, because they give many of the structural advantages of wood at a reduced cost.[10] In the 1980s OSB and flakeboard replaced plywood in much United States construction.[15] Manufactured homes described in the handbook have floor decking of particleboard, OSB or plywood, wall sheathing of fibreboard or OSB and roof decking of OSB or plywood.[16] The guidelines describe lightweight timber floors as typically having plywood or particleboard on the joists and gypsum plasterboard underneath.[17] In furniture, the office desks tested for the investigation of the 2001 World Trade Center fires had a 28 mm MDF core with a mean density of 820 kg/m³.[18]

Fire behaviour compared with solid wood

The basic processes are those of timber in fire. Unless the wood is green, its ignition can be modelled as four phases: drying, endothermic pyrolysis, exothermic pyrolysis and flaming combustion.[19] Panels differ from sawn timber in three ways that matter for fire. They are drier, they contain resins, and they are thin compared with their surface area.

Moisture is the first difference. Wood-based products and paper generally contain much less moisture than the wood they come from, which makes them easier to ignite and more combustible than solid wood.[4] Green wood can hold as much as 50 percent water by weight, and boiling off this water absorbs much of the heat of combustion.[20] Panel furnish is dried to low moisture contents before pressing, to help the glue bond.[21] Dry wood lacks the free water and much of the bound water, which gives it a significantly greater heat output in a fire.[20]

The binder is the second difference. Petroleum-derived resins complicate the fairly simple combustion chemistry of cellulose. Some contain aromatic rings, halogens or epoxies, which affect heat output, flame spread rate, smoke composition and smoke density.[5] Cone calorimeter data compiled by Tewarson (2002) give a chemical heat of combustion of 14.0 kJ/g for particleboard, fibreboard and MDF, and 10.7 kJ/g for melamine-faced particleboard.[22] The oxygen-bomb (gross) heat of combustion of hardboard is 19.9 MJ/kg, whereas wood in normal fires develops only about 12.5 MJ/kg.[23] For fire load calculations the guidelines give 18 MJ/kg for both particle board and wood.[24]

The adhesive also matters for integrity. Phenol-resorcinol and melamine adhesives are generally not affected by heat. For plywood and chipboard, however, the adhesive can make the difference between slow burning and a hazardous flash fire caused by delamination.[25] The research reviewed by Cholin (2008c) had not identified structural failures caused by the modern phenolic thermoset resins used in engineered wood components.[5]

Ignition and self-heating

Measured ignition properties of panels lie close to those of solid wood. A handbook table gives an ignition temperature of 390 °C and a critical ignition heat flux of 16 kW/m² for plywood, and 298 to 400 °C and 10 to 17 kW/m² for hardboard.[26] Quintiere (2002b) lists 382 °C for a 12.7 mm Douglas fir particleboard and 412 °C for a 12.7 mm stock particleboard.[27] As anchors, a wood particleboard ignited after about 250 s at 20 kW/m², and hardboard after about 150 s at 30 kW/m².[28] The critical heat flux depends on the correlation used to derive it, because it is extrapolated from test data to an infinite ignition time.[29] Another correlation gives only 6.4 to 10 kW/m² for chipboard and 8.5 to 10.6 kW/m² for plywood.[30]

For a thick panel under a constant radiant heat flux, the time to ignition increases with the thermal inertia kρc and with the square of the temperature rise needed. It decreases with the square of the heat flux in excess of the critical value. The correlation of Mikkola and Wichman, as given in NUREG-1805 after an SFPE engineering guide, is:[31]

tig=π4kρc(Tig−Ta)2(q˙′'r−q˙′'cr)2

Symbol Description Unit
tig Time to ignition s
kρc Thermal inertia (conductivity × density × specific heat) (kW/(m²·K))²·s
Tig Ignition temperature °C
Ta Ambient temperature °C
q˙′'r External (incident) heat flux kW/m²
q˙′'cr Critical heat flux for ignition kW/m²

The expression treats the panel as thermally thick, so the heated layer must stay thinner than the panel. The handbook calls a solid thermally thin only when temperature differences through it are essentially absent.[26] A characteristic heated depth is the square root of thermal diffusivity times time.[32] Plain plywood with a density of 540 kg/m³, a conductivity of 0.12 W/(m·K) and a specific heat of 2.5 kJ/(kg·K) has a diffusivity of about 8.9 × 10−8 m²/s.[33] Over the 68 s ignition time found in the example below, the heated depth is about 2.5 mm; over the handbook's 186 s it is about 4.1 mm. Both indicative depths are smaller than the 12.7 mm panel, so the thin-solid assumption in that example warrants caution. The thermal properties used for this depth check come from a separate plywood data set, not from the workbench itself.

A worked example in the handbook considers the 12.7 mm plywood end of a workbench, 2.0 m from the centre of a diesel pool fire. The incident heat flux of 22.6 kW/m² was doubled as a safety factor to 45.2 kW/m², and the net absorbed flux was assumed equal to this incident flux. With a density of 640 kg/m³, a specific heat of 2.8 kJ/(kg·K) and an ignition temperature of 390 °C, the handbook treats the panel as thermally thin. It finds an ignition time of 186 s, against 48 s for sprinkler activation, so fire spread beyond the pool fire was judged unlikely.[34] For the thick-solid correlation, NUREG-1805 supplies method-specific fitted properties rather than the physical thermal inertia from the separate property table.[35] Its fitted value is kρc = 0.54 for plain 12.7 mm plywood, alongside Tig = 390 °C and a critical flux of 16 kW/m², with Ta = 20 °C:[36]

tig=0.785×0.54×(390−20)2(45.2−16)2=0.424×136,900852.6≈68 s

For the 12.7 mm Douglas fir particleboard (kρc = 0.94, Tig = 382 °C, critical flux 16 kW/m²) the same calculation gives about 110 s. Both thick-solid estimates are longer than the 48 s sprinkler activation time, but the margin is much smaller than the thin-solid estimate suggests. The handbook itself warns that ignition is complex and that the limitations of such expressions are important.[26]

Panels can also ignite without a flame. Clean, dry wood products do not normally heat spontaneously at room temperature, but fibreboards heated at relatively moderate temperatures can start an exothermic reaction that leads to ignition.[37] Mitchell reported wood fibreboard that ignited after prolonged exposure to temperatures as low as 109 °C (229 °F).[38] Freshly made chipboard is stacked hot, and stacks of a few cubic metres can ignite within hours.[39] Fluorescent luminaires with ballasts should not be mounted directly on low-density cellulose fibreboard of 320 kg/m³ (20 lb/ft³) or less unless they are listed for it.[40]

Flame spread and heat release

In the United States, flame spread over wall and ceiling finishes is compared in the Steiner tunnel test (ASTM E84, UL 723 or NFPA 255). Ratings for virtually all wood-based panel products come from this test.[41] Red oak was the original reference material with a rating of 100, and most wood species fall between 90 and 160.[41] NFPA 101, as described in the 2008 handbook, groups wall and ceiling finishes by flame spread index. Class A covers 0 to 25, Class B 26 to 75 and Class C 76 to 200.[42]

Untreated panels mostly fall in Class C. Shaw (2008) gives flame spread indices of 115 to 130 for Douglas fir plywood, 95 for southern yellow pine plywood and 140 to 200 for particleboard.[6] The codes allow interior trim covering up to 10 percent of the wall or ceiling area to meet only Class C, because typical wood products achieve that class.[43] Low-density cellulosic fibreboard and acoustic ceiling tile were reported decades ago to reach indices of 225 to 350. Flame can spread over such linings as fast as people can run.[7] In 1982 two fire fighters died during live fire training in Boulder, Colorado, partly because of rapid fire spread across a low-density fibreboard ceiling.[44]

Range bars of flame spread index: plywood 95 to 130, particleboard 140 to 200, low-density fibreboard 225 to 350, treated panels below 25.
Flame spread indices of untreated and fire-retardant treated panels in the Steiner tunnel test, with the NFPA 101 classes A, B and C as described in 2008.

Thickness and mounting change the result. Thinner sections often spread flame faster than thicker ones, so products should be tested at the thickness and density in which they are used.[42] Wood panelling of 6.4 mm (0.25 in) or less spreads flame faster over furring strips with an air space than over a solid backing. Some codes therefore allow such thin Class B and C finishes only over a noncombustible substrate.[45] Untreated luan panelling, thin plywood panelling and pine boards on furring strips added to the severity of fires in fraternity buildings in Berkeley (1990) and Chapel Hill (1996) and in a Detroit board-and-care home (1992).[46]

In the ASTM E906 apparatus at 60 kW/m², wood products with about 8 percent moisture reached peak heat release rates of 90 to 170 kW/m². Their heat release rate increases linearly with density.[47] Karlsson and Quintiere give 124 kW/m² for Douglas fir plywood and 81 kW/m² for fire-retardant treated plywood.[48] In full-scale NIST tests, a wardrobe of 3.2 mm plywood peaked at 6,400 kW, one of 12.7 mm plywood at 3,100 kW and one of 19 mm particleboard at 1,900 kW. The particleboard unit released the most heat in total, 1,349 MJ, but flame spread over its thick panels was slower. Peak heat release rate depended inversely on panel thickness rather than on combustible mass.[49]

Bar chart of wardrobe peak heat release rate: 3.2 mm plywood 6,400 kW, 12.7 mm plywood 3,100 kW, 19 mm particleboard 1,900 kW.
Peak heat release rate of wardrobes of different panel constructions in NIST tests; the thinnest panels gave the highest peaks.

Fire resistance and charring

In the standard ASTM E119 fire resistance test, the surface of a wood panel ignites after about 2 minutes. It then chars at an average of about 0.85 mm/min for 8 minutes, after which the insulating char slows the rate to about 0.63 mm/min.[41] The base of the char layer is at about 287 °C, while 6.3 mm deeper the wood is at about 182 °C.[47] White (2002) gives a commonly used charring rate of 0.6 mm/min across the grain for solid timber. A constant rate is only reasonable while a panel is thick enough to act as a semi-infinite slab, and it rises once heat reaches the unexposed side.[50]

For the protective contribution of a panel to a timber assembly, White (2002) quotes an equation by Norén and Östman, based on data for various wood-based panel products. The contribution grows linearly with thickness, plus a small quadratic term that makes thicker panels slightly more effective per millimetre:[8]

bm=1.128t+0.0088t2

Symbol Description Unit
bm Contribution of the panel to the fire resistance of the assembly min
t Panel thickness mm

The equation applies to the ASTM E119 standard fire exposure. Panels of equal thickness still differed in fire resistance, depending on density, moisture content, type of adhesive and the structure of the panel.[8] As a worked example, an 18 mm panel gives 1.128 × 18 = 20.3 minutes from the linear term and 0.0088 × 18² = 2.85 minutes from the quadratic term, or about 23 minutes in total. A 9 mm panel gives about 10.9 minutes, so doubling the thickness slightly more than doubles the contribution.

Line chart of panel contribution to fire resistance rising from 0 to about 34 minutes as thickness rises from 0 to 25 mm.
Contribution of a wood-based panel to the fire resistance of an assembly under the ASTM E119 exposure, from the equation of Norén and Östman, with the 9 mm and 18 mm examples.

Older tabulated ratings in the handbook give similar orders of magnitude. Fir plywood on both faces of a hollow wall of nominal 2 by 4 in wood studs is credited with 10 minutes at 6.35 mm. The rating rises to 15 minutes at 9.53 mm, 20 minutes at 12.7 mm and 25 minutes at 15.9 mm.[51] A 12.7 mm fibreboard on one side of wood framing gives 5 minutes, or 10 minutes when flameproofed, against 15 minutes for 12.7 mm gypsum wallboard.[52]

Engineered joists made with panel webs raise a different concern. They have a larger surface area for their mass than sawn joists, so they burn faster and lose structural properties faster as they char.[5] Cholin (2008c) expects them to lose strength earlier in a fire than traditional sawn beams, although how much earlier had not been quantified.[19]

Fire-retardant treatment

Wood-based composite panels can be treated by chemical admixture, impregnation or coatings, each limited by its effect on the physical properties of the panel.[1] Fire-retardant particleboard and OSB are made by adding the chemicals before the board is formed. They give consistent flame spread and smoke-developed values when the chemical retention is consistent. Mixtures of alumina trihydrate, boric acid and wood fibres have produced panels with very low flame spread and smoke-developed values.[1]

Pressure impregnation of finished composite boards had not proved commercially feasible, partly because of losses in physical properties and inadequate fire retardancy.[1] Treatment at the wet pulp stage spreads the chemicals through the whole board. Wood-fibre acoustical tile and building panels made this way reach a flame spread index below 25.[9] Intumescent paints protect the exposed face of an existing board if they are maintained, but boards that swell and shrink with humidity can open untreated cracks.[53]

Shaw's table of tunnel results nevertheless lists pressure-impregnated particleboard, like treated plywood, with flame spread and smoke-developed indices below 25.[6] Fire-retardant plywood has an ignition temperature of 620 °C, and its flame spread was not measurable in the flame spread apparatus.[27] A 12.7 mm integrally treated particleboard reached a flame spread classification of 18. In a full-scale corner test with a wood crib it affected 25 percent of the wall and ceiling area, against 7 percent in control fires.[54] Treated lumber and plywood are covered under Fire-retardant-treated wood.

Regulation and classification

In the United States, the codes described by Hirschler (2008b) regulate panels as interior finish through the tunnel classes, with special rules for thin materials and finishes over air spaces.[45] Interior finish was the first item ignited in only about 6 percent of United States home fires in 1999 to 2002. Once a fire has grown, however, the finish can contribute extensively to its spread.[46]

New Zealand uses a classification based on heat release. In Verification Method C/VM2, lining materials receive a Group Number from 1 (best) to 4 (worst) according to the time to flashover in the ISO 9705 room test. In that test a 100 kW burner runs for 10 minutes and then 300 kW for a further 10 minutes.[55] The commentary to the first edition describes Group Number 3 materials as ordinary timber products that do not reach flashover within 2 minutes. Group Number 2 includes many fire-retardant treated timbers, with no flashover within 10 minutes.[55]

The first edition of C/VM2, as amended in December 2013, lets wood products at least 9.0 mm thick be taken as Group Number 3 without further testing. The density must be at least 600 kg/m³ for particle boards or 400 kg/m³ for other wood products. Any paint, varnish or stain must be no thicker than 0.4 mm and no heavier than 100 g/m².[56] Stored panels also form large fire loads: in a commentary example, 1,000 m³ of stored MDF holds about 11.5 TJ.[57]

See also

Notes

  1. ↑ 1.0 1.1 1.2 1.3 1.4 Shaw (2008), p. 6-137.
  2. ↑ 2.0 2.1 Cholin (2008c), pp. 6-65–6-66.
  3. ↑ 3.0 3.1 Cholin (2008c), p. 6-61.
  4. ↑ 4.0 4.1 4.2 Cholin (2008c), p. 6-65.
  5. ↑ 5.0 5.1 5.2 5.3 Cholin (2008c), p. 6-72.
  6. ↑ 6.0 6.1 6.2 6.3 Shaw (2008), p. 6-134.
  7. ↑ 7.0 7.1 McDaniel (2008), p. 20-186.
  8. ↑ 8.0 8.1 8.2 White (2002), p. 4-261.
  9. ↑ 9.0 9.1 Shaw (2008), p. 6-132.
  10. ↑ 10.0 10.1 10.2 Cholin (2008d), p. 9-8.
  11. ↑ Cholin (2008d), p. 9-7.
  12. ↑ Cholin (2008d), pp. 9-8–9-9.
  13. ↑ 13.0 13.1 Cholin (2008d), p. 9-9.
  14. ↑ National Research Council of Canada et al. (2005), pp. 3.4-4, 3.4-6.
  15. ↑ Cholin (2008c), p. 6-67.
  16. ↑ Paoletti (2008), pp. 20-64–20-65.
  17. ↑ National Research Council of Canada et al. (2005), p. 2.6-10.
  18. ↑ Ohlemiller et al. (2005), p. 71.
  19. ↑ 19.0 19.1 Cholin (2008c), p. 6-73.
  20. ↑ 20.0 20.1 Cholin (2008c), p. 6-64.
  21. ↑ Cholin (2008d), p. 9-6.
  22. ↑ Tewarson (2002), pp. 3-113, 3-115.
  23. ↑ Babrauskas (2008a), p. 6-280.
  24. ↑ National Research Council of Canada et al. (2005), p. 3.3-6.
  25. ↑ Pessiki (2008), p. 19-74.
  26. ↑ 26.0 26.1 26.2 Budnick et al. (2008), p. 3-159.
  27. ↑ 27.0 27.1 Quintiere (2002b), p. 2-251.
  28. ↑ Quintiere (1997), as cited in Iqbal and Salley (2004), p. 6-4.
  29. ↑ Iqbal and Salley (2004), p. 6-5.
  30. ↑ SFPE Engineering Guide (2002), as cited in Iqbal and Salley (2004), p. 6-12.
  31. ↑ SFPE Engineering Guide (2002), as cited in Iqbal and Salley (2004), p. 6-8.
  32. ↑ Van Rossum (2027), §5.2.
  33. ↑ Quintiere (1997), as cited in Iqbal and Salley (2004), p. 6-7.
  34. ↑ Budnick et al. (2008), pp. 3-163–3-165.
  35. ↑ Iqbal and Salley (2004), p. 6-7.
  36. ↑ SFPE Engineering Guide (2002), as cited in Iqbal and Salley (2004), pp. 6-10–6-11.
  37. ↑ Cholin (2008c), p. 6-69.
  38. ↑ Mitchell, as cited in Gore Willse (2008a), p. 10-31.
  39. ↑ Gray (2002), p. 2-224.
  40. ↑ Milatovich (2008), p. 8-157.
  41. ↑ 41.0 41.1 41.2 Cholin (2008c), p. 6-70.
  42. ↑ 42.0 42.1 Hirschler (2008b), p. 18-27.
  43. ↑ Hirschler (2008b), p. 18-36.
  44. ↑ Laughlin (2008), p. 12-172.
  45. ↑ 45.0 45.1 Hirschler (2008b), p. 18-38.
  46. ↑ 46.0 46.1 Hirschler (2008b), p. 18-37.
  47. ↑ 47.0 47.1 Cholin (2008c), p. 6-71.
  48. ↑ Karlsson and Quintiere (1999a), as cited in Iqbal and Salley (2004), p. 2-22.
  49. ↑ Babrauskas (2002b), p. 3-33.
  50. ↑ White (2002), pp. 4-260–4-261.
  51. ↑ Davis (2008b), p. 19-44.
  52. ↑ Davis (2008b), p. 19-45.
  53. ↑ Shaw (2008), p. 6-138.
  54. ↑ Benedetti and Colonna (2008), p. 6-226.
  55. ↑ 55.0 55.1 Ministry of Business, Innovation and Employment (2013), p. 141.
  56. ↑ Ministry of Business, Innovation and Employment (2013), p. 159B.
  57. ↑ Ministry of Business, Innovation and Employment (2013), p. 27.

References

  • Babrauskas, V. (2002b). Heat release rates. In P. J. DiNenno, D. Drysdale, C. L. Beyler, W. D. Walton, R. L. P. Custer, J. R. Hall Jr., & J. M. Watts Jr. (Eds.), SFPE handbook of fire protection engineering (3rd ed., pp. 3-1–3-37). National Fire Protection Association; Society of Fire Protection Engineers.
  • Babrauskas, V. (2008a). Tables and charts. In A. E. Cote, C. C. Grant, J. R. Hall Jr., & R. E. Solomon (Eds.), Fire protection handbook (20th ed., pp. 6-269–6-294). National Fire Protection Association.
  • Benedetti, R. P., & Colonna, G. R. (2008). Polymeric materials. In A. E. Cote, C. C. Grant, J. R. Hall Jr., & R. E. Solomon (Eds.), Fire protection handbook (20th ed., pp. 6-209–6-231). National Fire Protection Association.
  • Budnick, E. K., Hunt, S. P., & Wright, M. T. (2008). Closed form enclosure fire calculations. In A. E. Cote, C. C. Grant, J. R. Hall Jr., & R. E. Solomon (Eds.), Fire protection handbook (20th ed., pp. 3-145–3-166). National Fire Protection Association.
  • Cholin, J. M. (2008c). Wood and wood-based products. In A. E. Cote, C. C. Grant, J. R. Hall Jr., & R. E. Solomon (Eds.), Fire protection handbook (20th ed., pp. 6-61–6-74). National Fire Protection Association.
  • Cholin, J. M. (2008d). Woodworking facilities and processes. In A. E. Cote, C. C. Grant, J. R. Hall Jr., & R. E. Solomon (Eds.), Fire protection handbook (20th ed., pp. 9-3–9-25). National Fire Protection Association.
  • Davis, R. J. (2008b). Structural integrity during fire. In A. E. Cote, C. C. Grant, J. R. Hall Jr., & R. E. Solomon (Eds.), Fire protection handbook (20th ed., pp. 19-29–19-57). National Fire Protection Association.
  • Gore Willse, P. J. (2008a). Heating systems and appliances. In A. E. Cote, C. C. Grant, J. R. Hall Jr., & R. E. Solomon (Eds.), Fire protection handbook (20th ed., pp. 10-9–10-56). National Fire Protection Association.
  • Gray, B. (2002). Spontaneous combustion and self-heating. In P. J. DiNenno, D. Drysdale, C. L. Beyler, W. D. Walton, R. L. P. Custer, J. R. Hall Jr., & J. M. Watts Jr. (Eds.), SFPE handbook of fire protection engineering (3rd ed., pp. 2-211–2-228). National Fire Protection Association; Society of Fire Protection Engineers.
  • Hirschler, M. M. (2008b). Interior finish. In A. E. Cote, C. C. Grant, J. R. Hall Jr., & R. E. Solomon (Eds.), Fire protection handbook (20th ed., pp. 18-23–18-42). National Fire Protection Association.
  • Iqbal, N., & Salley, M. H. (2004). Fire Dynamics Tools (FDTs): Quantitative fire hazard analysis methods for the U.S. Nuclear Regulatory Commission Fire Protection Inspection Program (NUREG-1805). U.S. Nuclear Regulatory Commission, Office of Nuclear Reactor Regulation.
  • Laughlin, J. W. (2008). Training programs for fire and emergency service personnel. In A. E. Cote, C. C. Grant, J. R. Hall Jr., & R. E. Solomon (Eds.), Fire protection handbook (20th ed., pp. 12-161–12-175). National Fire Protection Association.
  • McDaniel, D. L. (2008). Library and museum collections. In A. E. Cote, C. C. Grant, J. R. Hall Jr., & R. E. Solomon (Eds.), Fire protection handbook (20th ed., pp. 20-179–20-202). National Fire Protection Association.
  • Milatovich, R. M. (2008). Electrical systems and appliances. In A. E. Cote, C. C. Grant, J. R. Hall Jr., & R. E. Solomon (Eds.), Fire protection handbook (20th ed., pp. 8-127–8-173). National Fire Protection Association.
  • Ministry of Business, Innovation and Employment. (2013). Commentary for Building Code clauses C1–C6 and Verification Method C/VM2.
  • National Research Council of Canada, International Code Council, Department of Building and Housing, & Australian Building Codes Board. (2005). International fire engineering guidelines (2005 ed.). Australian Building Codes Board.
  • Ohlemiller, T. J., Mulholland, G. W., Maranghides, A., Filliben, J. J., & Gann, R. G. (2005). Fire tests of single office workstations (NIST NCSTAR 1-5C). National Institute of Standards and Technology.
  • Paoletti, K. M. (2008). Manufactured housing. In A. E. Cote, C. C. Grant, J. R. Hall Jr., & R. E. Solomon (Eds.), Fire protection handbook (20th ed., pp. 20-63–20-71). National Fire Protection Association.
  • Pessiki, S. (2008). Analyzing structural fire damage. In A. E. Cote, C. C. Grant, J. R. Hall Jr., & R. E. Solomon (Eds.), Fire protection handbook (20th ed., pp. 19-65–19-76). National Fire Protection Association.
  • Quintiere, J. G. (2002b). Surface flame spread. In P. J. DiNenno, D. Drysdale, C. L. Beyler, W. D. Walton, R. L. P. Custer, J. R. Hall Jr., & J. M. Watts Jr. (Eds.), SFPE handbook of fire protection engineering (3rd ed., pp. 2-246–2-257). National Fire Protection Association; Society of Fire Protection Engineers.
  • Shaw, J. R. (2008). Fire-Retardant and flame-resistant treatment of cellulosic materials. In A. E. Cote, C. C. Grant, J. R. Hall Jr., & R. E. Solomon (Eds.), Fire protection handbook (20th ed., pp. 6-129–6-139). National Fire Protection Association.
  • Tewarson, A. (2002). Generation of heat and chemical compounds in fires. In P. J. DiNenno, D. Drysdale, C. L. Beyler, W. D. Walton, R. L. P. Custer, J. R. Hall Jr., & J. M. Watts Jr. (Eds.), SFPE handbook of fire protection engineering (3rd ed., pp. 3-82–3-161). National Fire Protection Association; Society of Fire Protection Engineers.
  • Van Rossum, E. (2027). Introduction to Fire Safety Engineering. Fire Safety Academy.
  • White, R. H. (2002). Analytical methods for determining fire resistance of timber members. In P. J. DiNenno, D. Drysdale, C. L. Beyler, W. D. Walton, R. L. P. Custer, J. R. Hall Jr., & J. M. Watts Jr. (Eds.), SFPE handbook of fire protection engineering (3rd ed., pp. 4-257–4-273). National Fire Protection Association; Society of Fire Protection Engineers.