Contents
The UL 94 flammability test is a family of small-flame laboratory tests that rank how plastic materials for parts of devices and appliances behave when a small gas flame is applied to them. It is published by Underwriters Laboratories as UL 94, Standard for Tests for Flammability of Plastic Materials for Parts in Devices and Appliances, and is one of the most widely used tests for plastics.[1] Its best-known results are the classes HB, V-2, V-1 and V-0, given here in increasing order of fire performance.[1]
The test does not measure a single fire property. Instead it combines aspects of ignitability, ease of extinction and flame spread in one procedure.[2] The most common versions use a 50 W flame about 20 mm high on a strip of plastic 125 mm long and 13 mm wide.[1] A material classed V-0 must stop burning in less than 10 seconds after the flame is removed and must not drop flaming particles that ignite cotton below it.[3][4] The test represents ignition by small electrical faults inside appliances reasonably well. It says little about behaviour in a room fire, and even a V-0 rating does not ensure that a material will not spread flame in a real fire.[5][4]
Purpose and scope
Most fire testing of products addresses reaction-to-fire properties: ignitability, ease of extinction, flame spread, smoke release, heat release and toxic gas release. Plastic materials are often assessed by a specific flammability test that combines ignitability, ease of extinction and flame spread, and UL 94 is that test.[2][1] Underwriters Laboratories has several standards for the ease of ignition and other characteristics of plastics used in products that it tests and lists or classifies, and UL 94 is a common one among them.[6]
The 50 W versions are most often used to characterise materials by their probability of being ignited by heat from electrical sources inside an appliance. For that scenario, the test gives an adequate picture of how plastic parts perform.[1] By extension, it is used as a simple way to compare plastics exposed to a low-intensity heat source. It also appears in specifications and material data sheets and serves as a tool for quality control and material development.[5] The NRC fire dynamics tools list UL 94 and the related ASTM methods among the empirical standard small-scale flammability tests.[7]
UL 94 is revised from time to time. Within the same handbook, Benedetti and Colonna list the 1991 edition, while Madrzykowski and Stroup cite the 1996 edition.[8][9] The details below describe the test as presented in the 2008 edition of the NFPA Fire Protection Handbook.
Test methods and classifications
UL 94 consists of several component tests. Each has an ASTM, IEC or ISO counterpart and leads to its own set of classes.[1] The flame size is given both as a nominal power and as a flame height.
| Test | Flame | Related methods | Classes |
|---|---|---|---|
| Horizontal burning test | 50 W (20 mm flame) | ASTM D635; IEC 60695-11-10 | HB |
| Vertical burning test | 50 W (20 mm flame) | ASTM D3801; IEC 60695-11-10 | V-0, V-1, V-2 |
| Vertical burning test, large flame | 500 W (125 mm flame) | ASTM D5048; IEC 60695-11-20 | 5VA, 5VB |
| Thin material vertical burning test | 50 W (20 mm flame) | ASTM D4804; ISO 9773 | VTM-0, VTM-1, VTM-2 |
| Horizontal burning test for foamed materials | 50 W (20 mm flame) | ASTM D4986; ISO 9772 | HF-1, HF-2, HBF |
The 50 W tests on solid plastics, which give the classes V-0, V-1, V-2 or HB, are the ones most frequently specified. They apply to specimens 125 mm long and 13 mm wide, with thicknesses of up to 3 mm.[1] The horizontal test observes the rate of burning along a flat specimen. In the vertical tests the strip is mounted upright, so that flame spreads upwards from the point of ignition.[6][3]
The 500 W flame of the 5V tests carries ten times the power of the standard flame. The thin material and foam versions cover nonrigid or thin flexible plastics and cellular materials, as the titles of the related ASTM and ISO methods show.[1] Benedetti and Colonna also describe UL 94 as including procedures for hot-wire and arc ignition, besides the rates of burning with the sample positioned horizontally and vertically.[6] Hirschler's list of component tests does not mention these ignition procedures.[1]
Vertical burning test
Procedure
The vertical burning test measures the resistance of a thin material to self-sustained ignition in an upward flame spread configuration. It is used to select materials for electronic devices and appliances.[3] A standard laboratory burner to ASTM D5025, run at a methane flow of 105 mL/min, produces a premixed methane-air flame of 50 W.[3] In a premixed flame the fuel and air are mixed before they reach the flame, as in a gas burner or a Bunsen burner.[10] The hottest part of a Bunsen burner flame reaches about 1,600 °C.[11]
The flame is applied for 10 seconds, which is meant to simulate a short ignition such as an electrical short circuit. The specimen, 125 mm long and 13 mm wide, is mounted 30 cm above a layer of loose cotton.[3] The criteria use the afterflame time, the time for which a specimen keeps flaming on its own after the test flame is removed. The cotton shows whether flaming particles or drops fall from the specimen.[3][4] A material is classified on the results of a set of five tests. If it fails any of the criteria, it receives a "V-fail" or "V-not" rating.[3]
Criteria
The three V classes differ in the permitted afterflame times and in whether the cotton may be ignited. The limits apply both to each specimen and to the total afterflame time of a condition set.[3][4]
| Class | Afterflame time of each specimen | Total afterflame time for any condition set | Cotton indicator |
|---|---|---|---|
| V-0 | less than 10 s | less than 50 s | not ignited |
| V-1 | less than 30 s | less than 250 s | not ignited |
| V-2 | less than 30 s | less than 250 s | ignited by flaming particles or drops |
V-0 is the strictest class, and V-1 and V-2 share the same time limits. The only difference between V-1 and V-2 is the cotton criterion.[4] V-2 therefore marks materials that pass the time limits but drip burning material. Hirschler ranks the four common classes, from best to worst, as V-0, V-1, V-2 and HB.[1]
Worked threshold check
The limits in the table are strict: a time of exactly 10 s reaches the V-0 boundary but does not meet its requirement of less than 10 s. That same duration is below the individual limit of 30 s for V-1 and V-2, although the total afterflame time for a condition set must also be less than 250 s. A time of exactly 30 s fails the individual limit for all three V classes. Among results that meet the V-1 and V-2 time limits, the cotton indicator determines which of those classes applies.[3][4] These checks apply the published thresholds; they do not represent measurements from a material or a complete UL 94 classification.
Why orientation and dripping matter
The vertical test is more demanding than the horizontal one because of how flames spread on a vertical surface. When a flame spreads upwards along a vertical surface, relatively much heat is transferred to the material above the burning part. That material is preheated, so the fire can spread faster.[10] A strip that burns slowly when lying flat may therefore burn readily when mounted upright. The same lesson appears in aviation. In the late 1960s and early 1970s, the fire resistance criteria for aircraft cabin materials moved from a horizontal Bunsen burner test to a requirement that a sample be self-extinguishing when tested vertically.[12]
The cotton criterion targets a typical property of thermoplastics. Thermoplastic articles tend to melt and flow when heated. In a fire this may let the material melt away from the flame front and stop burning. It may also produce flaming, tar-like drips that are difficult to extinguish and can start secondary fires.[13] UL 94 records both outcomes. A specimen that drips may extinguish quickly and still pass the time limits, but if its drips ignite the cotton the best class it can reach is V-2.[4]
Flame retardants act most strongly in the regime that UL 94 tests. They can be very effective in preventing ignition from low-level, short-duration flame and heat exposures, such as a 50 W flame applied for 10 seconds.[14][3] Phosphorus compounds promote char and an insulating glassy layer. Halogen compounds inhibit burning in the gas phase by interrupting chain reactions, and other retardants absorb heat by releasing water of hydration.[14] Fire retardants also raise the oxygen index substantially. Without them, common appliance plastics such as polypropylene (17.4), polystyrene (17.6 to 18.3) and ABS (18.3 to 18.8) have oxygen indices below the oxygen content of air.[15]
Use in specifications and regulation
The test fits its intended scenario, ignition of plastic parts by a small electrical source inside an appliance.[1] In the United States, as described by Hirschler (2008a), the test is also used for code compliance as an approval tool for light-transmitting plastics in building construction. Hirschler considers this use less justified.[5]
The semiconductor industry illustrates the risk of applying the classes outside their scope. Up to the year 2000, the industry followed Section 19 of SEMI S2-93, a prescriptive guideline with a limited scope for fire protection.[16] Most operators accepted UL 94 V-0, developed for small plastic appliances, to evaluate the combustibility of large polypropylene process tools. UL 94 V-0 was never intended for such tools, which can contain thousands of pounds of plastic and are often shielded from the building sprinklers.[16]
For cleanrooms, FM Global developed a far larger method, the parallel panel test of the ANSI FM 4910 protocol. Two panels 2.4 m high and 0.6 m wide face a sand burner that runs at a steady 60 kW for 20 minutes. The test is large enough that flame radiation dominates, as in most dangerous fires.[4] The 60 kW burner releases 1,200 times the power of the UL 94 flame. Tewarson describes the acceptance criteria of the 4910 protocol, both derived from tests in the fire propagation apparatus. The fire propagation index must not exceed 6 (m/s1/2)/(kW/m)2/3, and the smoke development index must not exceed 0.4 (g/g)(m/s1/2)/(kW/m)2/3.[17]
Limitations
The main limitation is scale. Madrzykowski and Stroup warn that even the V-0 class does not ensure that a material will not spread flames in a real fire. The 50 W flame, not 50 kW, represents a very small ignition source, and people unfamiliar with flammability may misread the ratings.[4]
An average living-room sofa fire reaches about 2.5 MW, which is 50,000 times the power of the test flame.[18] Larger flames do not simply heat harder. For ignition sources from a 0.3 kW Bunsen-type burner up to a 50 kW wastebasket, the peak heat flux stayed at about 30 to 40 kW/m². Only the heated area grew with the size of the source.[19]
The NFPA handbook states the same limits for small-scale plastics tests in general. The oxygen index test and UL 94 are now used mostly for product development and production control. With their small, low-intensity ignition sources, they are unsuitable for evaluating materials under room fire or other full-scale conditions.[20] Results of UL 94, like those of the ASTM plastics flammability tests, cannot be compared to the behaviour of materials in full-scale fires.[6] Hirschler adds that the test is unsuitable for fire safety engineering calculations.[5]
History shows how such ratings can mislead. Small-scale Bunsen burner tests were once used to label plastics as "self-extinguishing" or "nonburning" and therefore presumably safe, yet the same materials could show flash burning in real fires.[13] In aviation, the post-war horizontal Bunsen burner test created a widespread impression that cabin furnishings were fire resistive. They were not, and later research also revealed heavy smoke and toxic gas production.[12]
Flame retardants show the same limit from the material side. Under moderate exposures, retardants can greatly improve burning behaviour, but in severe exposures such as a fully developed room fire, treated and untreated plastics typically behave alike.[14] In NFPA sprinkler design for storage, fire-retardant modifiers are recognised to inhibit ignition, yet heat release once ignited is usually the same as for the unmodified plastic. Small-scale tests that measure relative horizontal burning rates are of little use for commodity classification, and intermediate-scale or full-scale testing is the best means to classify a modified material.[21][22]
Fire-retardant products can still bring large benefits in realistic fires. In tests at NIST, fire-retardant versions of products such as polystyrene television cabinets and polyphenylene oxide business machine housings reduced heat release, flame spread and the tendency to flashover. Potential escape times were reported to be 15 times longer, although the fire-retardant television cabinets produced twice as much total smoke.[14][23]
Related tests
UL 94 sits among several small-scale tests for plastics. The oxygen index test (ASTM D2863) measures the minimum oxygen concentration in a flowing oxygen and nitrogen mixture that supports candle-like downward burning. In practice it shows how easily a burning material is extinguished.[5] The glow wire tests (IEC 60695-2-10 and ASTM D6194) press an electrically heated wire against the material to simulate faults or overloads, and ASTM D3874 covers ignition by hot wire sources. Like the older ignition tests, the glow wire tests are of minor use for an engineering hazard assessment.[1]
For engineering use, Hirschler points to the critical heat flux for ignition. It is obtained by extrapolation from tests at several heat fluxes in apparatus such as the cone calorimeter or the fire propagation apparatus, and it can always be assessed. Data of this kind have value for fire safety engineering calculations and fire modelling.[1] A related horizontal method applies to vehicles. In the United States, the DOT motor vehicle safety standard, as described by Stull and Chines (2008), uses a Bunsen burner flame on a horizontal specimen. Materials in the occupant compartment may not transmit a flame front faster than 100 mm (4 in.) per minute, a test regarded as providing only minimum protection.[24]
See also
Notes
- ↑ 1.00 1.01 1.02 1.03 1.04 1.05 1.06 1.07 1.08 1.09 1.10 1.11 1.12 1.13 Hirschler (2008a), p. 6-41.
- ↑ 2.0 2.1 Hirschler (2008a), p. 6-40.
- ↑ 3.00 3.01 3.02 3.03 3.04 3.05 3.06 3.07 3.08 3.09 3.10 Madrzykowski and Stroup (2008), p. 2-42.
- ↑ 4.00 4.01 4.02 4.03 4.04 4.05 4.06 4.07 4.08 4.09 Madrzykowski and Stroup (2008), p. 2-43.
- ↑ 5.0 5.1 5.2 5.3 5.4 Hirschler (2008a), p. 6-42.
- ↑ 6.0 6.1 6.2 6.3 Benedetti and Colonna (2008), p. 6-228.
- ↑ Iqbal and Salley (2004), pp. C-17–C-18.
- ↑ Benedetti and Colonna (2008), p. 6-231.
- ↑ Madrzykowski and Stroup (2008), p. 2-47.
- ↑ 10.0 10.1 Van Rossum (2027), §4.3.
- ↑ Iqbal and Salley (2004), p. 3-9.
- ↑ 12.0 12.1 Boucher (2008), p. 21-139.
- ↑ 13.0 13.1 Benedetti and Colonna (2008), p. 6-225.
- ↑ 14.0 14.1 14.2 14.3 Benedetti and Colonna (2008), p. 6-229.
- ↑ Babrauskas (2008a), p. 6-282.
- ↑ 16.0 16.1 DeGiorgio and Peterkin (2008), p. 9-124.
- ↑ Tewarson (2002), p. 3-94.
- ↑ Van Rossum (2027), §4.5.
- ↑ Babrauskas (2002b), p. 3-6.
- ↑ Benedetti and Colonna (2008), p. 6-227.
- ↑ Golinveaux (2008), p. 16-72.
- ↑ Golinveaux (2008), p. 16-73.
- ↑ Benedetti and Colonna (2008), p. 6-230.
- ↑ Stull and Chines (2008), p. 6-98.
References
- Babrauskas, V. (2002b). Heat release rates. In P. J. DiNenno, D. Drysdale, C. L. Beyler, W. D. Walton, R. L. P. Custer, J. R. Hall Jr., & J. M. Watts Jr. (Eds.), SFPE handbook of fire protection engineering (3rd ed., pp. 3-1–3-37). National Fire Protection Association; Society of Fire Protection Engineers.
- Babrauskas, V. (2008a). Tables and charts. In A. E. Cote, C. C. Grant, J. R. Hall Jr., & R. E. Solomon (Eds.), Fire protection handbook (20th ed., pp. 6-269–6-294). National Fire Protection Association.
- Benedetti, R. P., & Colonna, G. R. (2008). Polymeric materials. In A. E. Cote, C. C. Grant, J. R. Hall Jr., & R. E. Solomon (Eds.), Fire protection handbook (20th ed., pp. 6-209–6-231). National Fire Protection Association.
- Boucher, B. (2008). Aviation. In A. E. Cote, C. C. Grant, J. R. Hall Jr., & R. E. Solomon (Eds.), Fire protection handbook (20th ed., pp. 21-135–21-149). National Fire Protection Association.
- DeGiorgio, V., & Peterkin, H. (2008). Semiconductor manufacturing. In A. E. Cote, C. C. Grant, J. R. Hall Jr., & R. E. Solomon (Eds.), Fire protection handbook (20th ed., pp. 9-119–9-129). National Fire Protection Association.
- Golinveaux, J. E. (2008). Sprinkler systems for storage facilities. In A. E. Cote, C. C. Grant, J. R. Hall Jr., & R. E. Solomon (Eds.), Fire protection handbook (20th ed., pp. 16-71–16-89). National Fire Protection Association.
- Hirschler, M. M. (2008a). Concepts and protocols of fire testing. In A. E. Cote, C. C. Grant, J. R. Hall Jr., & R. E. Solomon (Eds.), Fire protection handbook (20th ed., pp. 6-35–6-60). National Fire Protection Association.
- Iqbal, N., & Salley, M. H. (2004). Fire Dynamics Tools (FDTs): Quantitative fire hazard analysis methods for the U.S. Nuclear Regulatory Commission Fire Protection Inspection Program (NUREG-1805). U.S. Nuclear Regulatory Commission, Office of Nuclear Reactor Regulation.
- Madrzykowski, D., & Stroup, D. W. (2008). Flammability hazard of materials. In A. E. Cote, C. C. Grant, J. R. Hall Jr., & R. E. Solomon (Eds.), Fire protection handbook (20th ed., pp. 2-31–2-48). National Fire Protection Association.
- Stull, J. O., & Chines, S. A. (2008). Fibers and textiles. In A. E. Cote, C. C. Grant, J. R. Hall Jr., & R. E. Solomon (Eds.), Fire protection handbook (20th ed., pp. 6-75–6-102). National Fire Protection Association.
- Tewarson, A. (2002). Generation of heat and chemical compounds in fires. In P. J. DiNenno, D. Drysdale, C. L. Beyler, W. D. Walton, R. L. P. Custer, J. R. Hall Jr., & J. M. Watts Jr. (Eds.), SFPE handbook of fire protection engineering (3rd ed., pp. 3-82–3-161). National Fire Protection Association; Society of Fire Protection Engineers.
- Van Rossum, E. (2027). Introduction to Fire Safety Engineering. Fire Safety Academy.