Line 14: Line 14:


Four theories explain how fire retardants act, and in most cases more than one mechanism is involved. Thermal theories hold that the chemicals conduct heat away, absorb heat or, most importantly, insulate the wood. Coating theories hold that some retardants melt or foam into a layer that excludes oxygen and holds back combustible gases. Gas theories hold that others release nonflammable gases such as water, ammonia and carbon dioxide, or inhibit the free-radical reactions of the flame.<ref name="Shaw-6-130" /> The chemical theory holds that treated cellulose forms fewer liquids and flammable gases and more solid char.<ref name="Shaw-6-131" />
Four theories explain how fire retardants act, and in most cases more than one mechanism is involved. Thermal theories hold that the chemicals conduct heat away, absorb heat or, most importantly, insulate the wood. Coating theories hold that some retardants melt or foam into a layer that excludes oxygen and holds back combustible gases. Gas theories hold that others release nonflammable gases such as water, ammonia and carbon dioxide, or inhibit the free-radical reactions of the flame.<ref name="Shaw-6-130" /> The chemical theory holds that treated cellulose forms fewer liquids and flammable gases and more solid char.<ref name="Shaw-6-131" />
[[File:fse-fire-retardant-treated-wood-v4.svg|thumb|upright=1.5|alt=Two flow sketches: untreated cellulose gives mostly liquids and flammable gases; treated cellulose gives mostly char and little flammable gas.|Burning sequence of untreated (left) and fire-retardant treated (right) cellulose; circle sizes indicate the relative amounts of products. Based on Shaw (2008), pp. 6-130–6-131.]]


Studies at the United States Forest Products Laboratory quantified the chemical effect. Pyrolysis of the lignin in wood starts at about 220 °C and that of the cellulose near 270 °C. Fire-retardant chemicals often lower the start of cellulose decomposition from 270 to 230 °C and drive it directly towards char and water instead of flammable gases and tars.<ref name="Shaw-6-131" /> At 360 °C the char yield from cellulose rises from 15 percent to 30 to 35 percent, and the char yield from lignin rises from 49 to 57 percent. Combustion of wood has two exothermic stages: flaming near 330 °C as the cellulose decomposes, and glowing near 430 °C as the lignin char oxidises. Fire retardants greatly reduce the first, and some chemicals also reduce the second.<ref name="Shaw-6-131" />
Studies at the United States Forest Products Laboratory quantified the chemical effect. Pyrolysis of the lignin in wood starts at about 220 °C and that of the cellulose near 270 °C. Fire-retardant chemicals often lower the start of cellulose decomposition from 270 to 230 °C and drive it directly towards char and water instead of flammable gases and tars.<ref name="Shaw-6-131" /> At 360 °C the char yield from cellulose rises from 15 percent to 30 to 35 percent, and the char yield from lignin rises from 49 to 57 percent. Combustion of wood has two exothermic stages: flaming near 330 °C as the cellulose decomposes, and glowing near 430 °C as the lignin char oxidises. Fire retardants greatly reduce the first, and some chemicals also reduce the second.<ref name="Shaw-6-131" />
Line 23: Line 24:


The wood is loaded into a cylinder up to 2.5 m in diameter and more than 43 m long. A vacuum first draws much of the air out of the wood cells. The cylinder is then filled with the treating solution, and the pressure is raised to as much as 1,379 kPa (200 psi) to force chemical into the empty voids. The process can be run to refusal, the point at which the wood absorbs no more solution.<ref name="Shaw-6-133" /> After a final vacuum to remove surface chemical, the charge is dried and is ready for use. In the manufacturing practice described by Shaw (2008), pressure impregnation is done by a licensed treater after the wood has been cut to size.<ref name="Shaw-6-134" />
The wood is loaded into a cylinder up to 2.5 m in diameter and more than 43 m long. A vacuum first draws much of the air out of the wood cells. The cylinder is then filled with the treating solution, and the pressure is raised to as much as 1,379 kPa (200 psi) to force chemical into the empty voids. The process can be run to refusal, the point at which the wood absorbs no more solution.<ref name="Shaw-6-133" /> After a final vacuum to remove surface chemical, the charge is dried and is ready for use. In the manufacturing practice described by Shaw (2008), pressure impregnation is done by a licensed treater after the wood has been cut to size.<ref name="Shaw-6-134" />
[[File:fse-fire-retardant-treated-wood-v1.svg|thumb|upright=1.5|alt=Five-step flow: wood loaded into a cylinder, vacuum, solution filled, pressure up to 1,379 kPa, drained and dried.|The pressure impregnation cycle for fire-retardant-treated wood: vacuum, filling, pressure up to 1,379 kPa (200 psi), draining, final vacuum and drying. Based on Shaw (2008), p. 6-133.]]


The advantages are a large, closely controlled and uniform chemical load, test samples that are easy to obtain and a treatment that can be considered permanent under normal conditions of use. Nonleachable treatments should be chosen for exterior use, and treatments with low hygroscopicity for humid interiors.<ref name="Shaw-6-133" /> Plywood can be fully treated when appearance is unimportant, and it then generally has a flame spread index below 25. Where a natural face is wanted, untreated face veneers are laminated onto treated cores, giving indices of about 20 to 75 that vary roughly inversely with the density of the face veneer.<ref name="Shaw-6-135" /> Fire-retardant particleboard and OSB are made by adding the chemicals before the board is formed, as described under [[Wood-based panel products]].<ref name="Shaw-6-137">Shaw (2008), p. 6-137.</ref>
The advantages are a large, closely controlled and uniform chemical load, test samples that are easy to obtain and a treatment that can be considered permanent under normal conditions of use. Nonleachable treatments should be chosen for exterior use, and treatments with low hygroscopicity for humid interiors.<ref name="Shaw-6-133" /> Plywood can be fully treated when appearance is unimportant, and it then generally has a flame spread index below 25. Where a natural face is wanted, untreated face veneers are laminated onto treated cores, giving indices of about 20 to 75 that vary roughly inversely with the density of the face veneer.<ref name="Shaw-6-135" /> Fire-retardant particleboard and OSB are made by adding the chemicals before the board is formed, as described under [[Wood-based panel products]].<ref name="Shaw-6-137">Shaw (2008), p. 6-137.</ref>
Line 28: Line 30:
== Fire performance ==
== Fire performance ==
The tunnel test shows the largest effect. In Shaw's table, untreated lumber ranges from a [[flame spread index]] of 60 to 70 for hemlock to 130 to 195 for southern yellow pine. Douglas fir plywood reaches 115 to 130 and particleboard 140 to 200. After pressure impregnation every listed product has a flame spread index and a smoke-developed index below 25.<ref name="Shaw-6-134" /> Under NFPA 101, as described in the 2008 edition of the handbook, this moves the material from Class B or C into Class A, which covers indices of 0 to 25.<ref name="Hirschler-18-27">Hirschler (2008b), p. 18-27.</ref>
The tunnel test shows the largest effect. In Shaw's table, untreated lumber ranges from a [[flame spread index]] of 60 to 70 for hemlock to 130 to 195 for southern yellow pine. Douglas fir plywood reaches 115 to 130 and particleboard 140 to 200. After pressure impregnation every listed product has a flame spread index and a smoke-developed index below 25.<ref name="Shaw-6-134" /> Under NFPA 101, as described in the 2008 edition of the handbook, this moves the material from Class B or C into Class A, which covers indices of 0 to 25.<ref name="Hirschler-18-27">Hirschler (2008b), p. 18-27.</ref>
[[File:fse-fire-retardant-treated-wood-v2.svg|thumb|upright=1.5|alt=Paired bars per wood product: untreated flame spread index 60 to 200, all treated values below 25 in the Class A band.|Flame spread index of untreated and pressure-impregnated lumber and panels in the tunnel test (NFPA 255, ASTM E84), with the NFPA 101 classes as described in 2008. Based on Shaw (2008), p. 6-134 and Hirschler (2008b), p. 18-27.]]


Heat release tests also report lower values for treated plywood. Karlsson and Quintiere give heat release rates per unit area of 124 kW/m² for Douglas fir plywood and 81 kW/m² for fire-retardant treated plywood, a reduction of about 35 percent.<ref name="Iqbal-2-22">Karlsson and Quintiere (1999a), as cited in Iqbal and Salley (2004), p. 2-22.</ref>
Heat release tests also report lower values for treated plywood. Karlsson and Quintiere give heat release rates per unit area of 124 kW/m² for Douglas fir plywood and 81 kW/m² for fire-retardant treated plywood, a reduction of about 35 percent.<ref name="Iqbal-2-22">Karlsson and Quintiere (1999a), as cited in Iqbal and Salley (2004), p. 2-22.</ref>
Line 60: Line 63:


For this worked example, the model estimates ignition after about 30 s for plain plywood and 839 s (about 14 min) for treated plywood at 60 kW/m². At or below 44 kW/m², it predicts no ignition of the treated specimen under its constant-flux assumptions; this does not establish immunity in a real fire. Close to the critical flux the result is very sensitive to the fitted properties, so it should be read as an order-of-magnitude estimate. The handbook warns that ignition is a complex phenomenon and that the limitations of such expressions are important.<ref name="Budnick-3-159">Budnick et al. (2008), p. 3-159.</ref>
For this worked example, the model estimates ignition after about 30 s for plain plywood and 839 s (about 14 min) for treated plywood at 60 kW/m². At or below 44 kW/m², it predicts no ignition of the treated specimen under its constant-flux assumptions; this does not establish immunity in a real fire. Close to the critical flux the result is very sensitive to the fitted properties, so it should be read as an order-of-magnitude estimate. The handbook warns that ignition is a complex phenomenon and that the limitations of such expressions are important.<ref name="Budnick-3-159">Budnick et al. (2008), p. 3-159.</ref>
[[File:fse-fire-retardant-treated-wood-v3.svg|thumb|upright=1.5|alt=Line chart of time to ignition against heat flux; untreated plywood curve near 30 s at 60 kW/m², treated curve near 840 s, rising steeply towards 44 kW/m².|Estimated time to ignition of 12.7 mm untreated and fire-retardant plywood against incident heat flux, from the correlation of Mikkola and Wichman. Based on Iqbal and Salley (2004), pp. 6-8 and 6-10–6-11.]]


The treatment does much less for charring and fire resistance. White (2002) notes that fire retardants are designed to reduce flame spread and may only slightly increase the time until the wood ignites. Some lower the temperature at which charring occurs, which may increase the [[charring rate]], while a few have been found to improve charring resistance.<ref name="White-4-261">White (2002), p. 4-261.</ref> Shaw (2008) likewise states that only some fire-retardant coatings significantly increase the resistance of wood to sustained fire exposure or delay the loss of its load-bearing capacity.<ref name="Shaw-6-132" />
The treatment does much less for charring and fire resistance. White (2002) notes that fire retardants are designed to reduce flame spread and may only slightly increase the time until the wood ignites. Some lower the temperature at which charring occurs, which may increase the [[charring rate]], while a few have been found to improve charring resistance.<ref name="White-4-261">White (2002), p. 4-261.</ref> Shaw (2008) likewise states that only some fire-retardant coatings significantly increase the resistance of wood to sustained fire exposure or delay the loss of its load-bearing capacity.<ref name="Shaw-6-132" />

Revision as of 07:52, 8 November 2026

Fire-retardant-treated wood (FRTW) is lumber, plywood or another wood product that has been impregnated with fire-retardant chemicals, usually by a vacuum and pressure process during manufacture, so that flame spreads slowly over its surface. In the United States code terminology described by Shaw (2008), the term has a test-based meaning. Tested in the Steiner tunnel for 30 minutes instead of the usual 10, the product must keep a flame spread index of 25 or less, without progressive combustion.[1][2]

The chemicals change the way cellulose decomposes, so that more char and water and fewer flammable gases are formed.[3] In the tests summarised by Shaw (2008), treatment lowered heat release and a treated plywood lining did not reach flashover under a specified burner exposure, while an untreated lining did.[4] FRTW is still combustible. No treatment makes wood noncombustible, and pressure impregnation does not by itself give a fire resistance rating.[5][6] Some formulations of the 1980s weakened plywood roof sheathing in hot attics, which led to new test standards and reformulated chemicals.[7]

Definition and terminology

The definition quoted by Shaw (2008), after NFPA 255 (ASTM E84), has three parts. FRTW is any wood product impregnated with chemicals by a pressure process or other means during manufacture. When tested for 30 minutes, it must have a flame spread of not over 25 and show no evidence of progressive combustion. The flame front must also never progress more than 3.20 m (10½ ft) beyond the centreline of the burner during the test.[1] The standard tunnel test runs for 10 minutes, so the definition triples the test duration.[2] In the United States, pressure-impregnated and coating treatments are covered by NFPA 703, Standard for Fire Retardant–Treated Wood and Fire-Retardant Coatings for Building Materials, as described in the 2008 edition of the handbook.[5]

The words used for treated materials are often confused. Shaw (2008) reserves fire resistant for the ability of a structure, material or assembly to resist a large-scale severe fire, measured as a fire resistance rating in the NFPA 251 (ASTM E119) test.[8] Fire retardant signifies a lesser degree of protection and refers to chemicals, treatments or coatings that reduce the combustibility of building materials. Flame retardant is the preferred term for treatments of decorative materials such as fabrics and foliage, and fireproof and flameproof are described as misleading.[8][6] The chemistry of the additives themselves is covered under Flame retardant.

A common misconception is that every fire-retardant treatment gives a fire resistance rating. Some fire-resistive coatings can improve the fire endurance of combustible assemblies, but other treatments only slow the rate of burning and the rate at which the treated material adds fuel to a fire.[6] The treatments also have practical limits. They are not all permanent, they cannot make cellulosic materials noncombustible, they affect other properties of the wood and they add cost.[6]

How the treatment works

Wood does not burn directly. When heated it pyrolyses into gases, vapours and mists that can form flammable mixtures with air and burn as visible flames. The charcoal left behind can burn separately by combining directly with oxygen, which is seen as glowing.[6] This distinction matters, because many chemicals that inhibit flaming have little or no effect on flameless combustion or afterglow. The general behaviour of untreated wood is described under Timber in fire.

Four theories explain how fire retardants act, and in most cases more than one mechanism is involved. Thermal theories hold that the chemicals conduct heat away, absorb heat or, most importantly, insulate the wood. Coating theories hold that some retardants melt or foam into a layer that excludes oxygen and holds back combustible gases. Gas theories hold that others release nonflammable gases such as water, ammonia and carbon dioxide, or inhibit the free-radical reactions of the flame.[6] The chemical theory holds that treated cellulose forms fewer liquids and flammable gases and more solid char.[3]

Two flow sketches: untreated cellulose gives mostly liquids and flammable gases; treated cellulose gives mostly char and little flammable gas.
Burning sequence of untreated (left) and fire-retardant treated (right) cellulose; circle sizes indicate the relative amounts of products. Based on Shaw (2008), pp. 6-130–6-131.

Studies at the United States Forest Products Laboratory quantified the chemical effect. Pyrolysis of the lignin in wood starts at about 220 °C and that of the cellulose near 270 °C. Fire-retardant chemicals often lower the start of cellulose decomposition from 270 to 230 °C and drive it directly towards char and water instead of flammable gases and tars.[3] At 360 °C the char yield from cellulose rises from 15 percent to 30 to 35 percent, and the char yield from lignin rises from 49 to 57 percent. Combustion of wood has two exothermic stages: flaming near 330 °C as the cellulose decomposes, and glowing near 430 °C as the lignin char oxidises. Fire retardants greatly reduce the first, and some chemicals also reduce the second.[3]

The chemicals commonly used in the past included monobasic and dibasic ammonium phosphates, ammonium sulfate, borax, boric acid, zinc chloride and sodium dichromate, usually in combination. Newer formulations tend to leave out hygroscopic salts such as ammonium sulfate and zinc chloride, and some include organophosphorus compounds and amino resins.[5][1] The cited newer formulations improved tolerance of relative humidities up to 95 percent; nonleachable formulations can also be used outdoors.[1]

Pressure impregnation

Pressure impregnation is used for relatively dense, nonabsorbent materials such as wood. It replaces the air in the wood cells with a chemical solution, which leaves the chemicals behind as it dries. The fire-retarding effect is directly related to the amount of chemical deposited per unit volume and to the depth of penetration.[5][1] Shaw (2008) illustrates this with a fence 3.05 m high and 15.25 m long of nominal 25 mm pine boards. Brushing applies about 15 L of solution and leaves the flame spread index between 130 and 195. Impregnating the same boards to refusal deposits about 852 L and cuts the index to below 25.[1]

The wood is loaded into a cylinder up to 2.5 m in diameter and more than 43 m long. A vacuum first draws much of the air out of the wood cells. The cylinder is then filled with the treating solution, and the pressure is raised to as much as 1,379 kPa (200 psi) to force chemical into the empty voids. The process can be run to refusal, the point at which the wood absorbs no more solution.[1] After a final vacuum to remove surface chemical, the charge is dried and is ready for use. In the manufacturing practice described by Shaw (2008), pressure impregnation is done by a licensed treater after the wood has been cut to size.[7]

Five-step flow: wood loaded into a cylinder, vacuum, solution filled, pressure up to 1,379 kPa, drained and dried.
The pressure impregnation cycle for fire-retardant-treated wood: vacuum, filling, pressure up to 1,379 kPa (200 psi), draining, final vacuum and drying. Based on Shaw (2008), p. 6-133.

The advantages are a large, closely controlled and uniform chemical load, test samples that are easy to obtain and a treatment that can be considered permanent under normal conditions of use. Nonleachable treatments should be chosen for exterior use, and treatments with low hygroscopicity for humid interiors.[1] Plywood can be fully treated when appearance is unimportant, and it then generally has a flame spread index below 25. Where a natural face is wanted, untreated face veneers are laminated onto treated cores, giving indices of about 20 to 75 that vary roughly inversely with the density of the face veneer.[4] Fire-retardant particleboard and OSB are made by adding the chemicals before the board is formed, as described under Wood-based panel products.[9]

Fire performance

The tunnel test shows the largest effect. In Shaw's table, untreated lumber ranges from a flame spread index of 60 to 70 for hemlock to 130 to 195 for southern yellow pine. Douglas fir plywood reaches 115 to 130 and particleboard 140 to 200. After pressure impregnation every listed product has a flame spread index and a smoke-developed index below 25.[7] Under NFPA 101, as described in the 2008 edition of the handbook, this moves the material from Class B or C into Class A, which covers indices of 0 to 25.[10]

Paired bars per wood product: untreated flame spread index 60 to 200, all treated values below 25 in the Class A band.
Flame spread index of untreated and pressure-impregnated lumber and panels in the tunnel test (NFPA 255, ASTM E84), with the NFPA 101 classes as described in 2008. Based on Shaw (2008), p. 6-134 and Hirschler (2008b), p. 18-27.

Heat release tests also report lower values for treated plywood. Karlsson and Quintiere give heat release rates per unit area of 124 kW/m² for Douglas fir plywood and 81 kW/m² for fire-retardant treated plywood, a reduction of about 35 percent.[11]

In a room fire test with a burner exposure of 40 kW for 5 minutes and then 160 kW for 5 minutes, untreated Douglas fir plywood linings reached flashover after 3.3 minutes. Their maximum heat release rate was 7.3 MW. Pressure-impregnated plywood did not reach flashover, and its maximum heat release rate was 0.6 MW. The maximum smoke optical density fell from 1.11 to 0.76.[4]

Ignition properties change as well. A handbook table gives fire-retardant plywood an ignition temperature of 620 °C and a critical ignition heat flux of 44 kW/m², against 390 °C and 16 kW/m² for ordinary plywood.[12] In the flame spread data compiled by Quintiere (2002b), flame spread over 12.7 mm fire-retardant plywood was not measurable.[13] The correlation of Mikkola and Wichman estimates the ignition time of a thick solid from its thermal inertia kρc, its ignition temperature and the heat flux above the critical value:[14]

tig=π4kρc(Tig−Ta)2(q˙′'r−q˙′'cr)2

Symbol Description Unit
tig Time to ignition s
kρc Thermal inertia (conductivity × density × specific heat) (kW/(m²·K))²·s
Tig Ignition temperature °C
Ta Ambient temperature °C
q˙′'r External (incident) heat flux kW/m²
q˙′'cr Critical heat flux for ignition kW/m²

The correlation applies to thermally thick specimens under a constant radiant heat flux above the critical value, and it predicts no ignition at or below that value under those assumptions. The tabulated inputs are method-specific fitted properties, rather than independent measurements of thermal inertia.[15] As a worked example, the fitted value of kρc for 12.7 mm plywood is 0.54, with Tig = 390 °C and a minimum flux of 16 kW/m². For 12.7 mm fire-retardant plywood the respective values are 0.76, 620 °C and 44 kW/m².[16] At an incident heat flux of 60 kW/m² and an ambient temperature of 20 °C:

tig,untreated=0.424×(390−20)2(60−16)2=0.424×136,9001,936≈30 s

tig,FR=0.597×(620−20)2(60−44)2=0.597×360,000256≈839 s

For this worked example, the model estimates ignition after about 30 s for plain plywood and 839 s (about 14 min) for treated plywood at 60 kW/m². At or below 44 kW/m², it predicts no ignition of the treated specimen under its constant-flux assumptions; this does not establish immunity in a real fire. Close to the critical flux the result is very sensitive to the fitted properties, so it should be read as an order-of-magnitude estimate. The handbook warns that ignition is a complex phenomenon and that the limitations of such expressions are important.[12]

Line chart of time to ignition against heat flux; untreated plywood curve near 30 s at 60 kW/m², treated curve near 840 s, rising steeply towards 44 kW/m².
Estimated time to ignition of 12.7 mm untreated and fire-retardant plywood against incident heat flux, from the correlation of Mikkola and Wichman. Based on Iqbal and Salley (2004), pp. 6-8 and 6-10–6-11.

The treatment does much less for charring and fire resistance. White (2002) notes that fire retardants are designed to reduce flame spread and may only slightly increase the time until the wood ignites. Some lower the temperature at which charring occurs, which may increase the charring rate, while a few have been found to improve charring resistance.[17] Shaw (2008) likewise states that only some fire-retardant coatings significantly increase the resistance of wood to sustained fire exposure or delay the loss of its load-bearing capacity.[5]

Strength, durability and toxicity

Early formulations were very hygroscopic and corroded metal fasteners. In the late 1980s producers changed to low-hygroscopicity formulations that greatly improved corrosion resistance. There were then reports of structural failures in fire-retardant treated plywood roofs under high temperature and humidity.[1] Forest Products Laboratory research showed that acidic chemicals such as monoammonium phosphate can degrade wood and reduce its strength above 66 °C (150 °F) in humid conditions, as found in attics.[7] Some codes had required a 1.2 m (4 ft) strip of treated plywood along each side of a fire wall. Some of these chemicals reacted with heat and humidity and destroyed the plywood, and thousands of roofs had to be replaced.[18]

The affected formulations were modified and retested to new ASTM methods for the properties and mechanical properties of fire-retardant treated softwood plywood exposed to elevated temperatures. These reformulations greatly reduced the strength losses, and at least one new formulation achieves good flame spread performance without phosphates.[7] Cholin (2008c) adds that fire-retardant treatment may make plywood sheathing and structural lumber brittle. Suggested causes include chemical attack on the cellulose fibres and the high temperatures used to redry the wood after treatment. Building codes provide for derating the strength of treated members.[19]

In the combustion-toxicity tests summarised by Shaw (2008), smoke from treated wood was reported to be no more toxic than smoke from untreated Douglas fir. Some treatments nevertheless released minor amounts of toxicants other than carbon monoxide. Treated and untreated wood products tested by the University of Pittsburgh method ranged in LC50 from 7 to 72 g, and radiant furnace tests found smoke from treated wood slightly less toxic.[4] Janssens (2002) explains why gas yield alone does not determine toxic hazard. Some fire-retardant treatments increase the yield of toxic gases but greatly reduce the mass loss rate; the lower mass loss can reduce toxic gas release in a given fire scenario.[20]

Testing and coatings

Treated wood is evaluated by several methods. The Steiner tunnel gives the flame spread and smoke-developed indices on which listings are based. A room test for wall and ceiling materials, developed at the National Institute of Standards and Technology and standardised as ISO 9705, is used for treated panel products.[7] The cone calorimeter (ASTM E1354) and the intermediate scale calorimeter (ASTM E1623) distinguish the burning rates of treated and untreated wood. Correlations between cone, room and tunnel results have been somewhat successful.[7] In the cone calorimeter, some highly fire-retardant treated materials give off vapours that tend to put out the pilot flame, so the igniter must be designed for this.[21]

Where impregnation is impracticable, as in existing buildings, fire-retardant coatings can be brushed, rolled, sprayed or trowelled onto the wood.[4] Underwriters Laboratories requires a listed coating to reach a flame spread rating of 50 or less, or a 50 percent reduction from the untreated surface, whichever is lower.[22] The four types are intumescent paints, mastics, gas-forming paints and cementitious or mineral-fibre coatings. Coatings can be applied in place, are relatively cheap and do not cause strength loss. Their drawbacks are thin applications, untreatable hidden surfaces, limited life, damage and the need for maintenance, and their use outdoors is questionable.[22]

Treatments also matter for roofs and exteriors. Coating wood shingles in place has not proved practical, but shingles impregnated with a fire-retardant solution are more durable and carry a Class B or C roof covering rating.[23] Water-based gels applied to wood siding raised the time to ignition at 25 kW/m² from 30 s to about 300 s, but only as temporary protection against wildland fire.[22] Oil-type preservatives such as creosote increase the fire hazard of wood. Borates, in contrast, act as both preservative and fire retardant.[9]

Use in building regulation

In the United States, the model codes described by Shaw (2008) allow fire-retardant-treated wood in noncombustible construction, with some limitations.[7] Shaw also lists as a misuse the promotion of pressure-impregnated wood where noncombustible materials are absolutely required, because even the best treatments still contribute some fuel and smoke. At the time, ASTM and ISO were considering a "limited combustibility classification" based on heat release rate, and FRTW was given as a material that could be so classified.[24] The related United States category is described under Limited-combustible material. Miller and Roether (2008) likewise recommend that exhibition booths be built of noncombustible, limited-combustible or fire-retardant-treated materials.[25]

Older city codes made similar allowances. The 1968 Building Code of the City of New York, applied to the World Trade Center towers, permitted fire retardant treated wood complying with its Section C26-502.6 in some non-bearing construction elements.[26] In the February 1975 fire in WTC 1, the fire-retardant treated wood paneling on the telephone closet walls of the 10th and 12th floors was destroyed with virtually all other combustibles.[27]

In New Zealand, the commentary to the first edition of Verification Method C/VM2 (2013) groups lining materials by their time to flashover in the ISO 9705 room test. It names many fire-retardant treated timbers as typical Group Number 2 materials, with no flashover within 10 minutes. Ordinary timber products are typical Group Number 3 materials, with no flashover within 2 minutes.[28] The commentary adds that actual performance depends on composition, thickness and additives, and must be verified by test.[28]

See also

Notes

  1. ↑ 1.0 1.1 1.2 1.3 1.4 1.5 1.6 1.7 1.8 Shaw (2008), p. 6-133.
  2. ↑ 2.0 2.1 Hirschler (2008b), p. 18-26.
  3. ↑ 3.0 3.1 3.2 3.3 Shaw (2008), p. 6-131.
  4. ↑ 4.0 4.1 4.2 4.3 4.4 Shaw (2008), p. 6-135.
  5. ↑ 5.0 5.1 5.2 5.3 5.4 Shaw (2008), p. 6-132.
  6. ↑ 6.0 6.1 6.2 6.3 6.4 6.5 Shaw (2008), p. 6-130.
  7. ↑ 7.0 7.1 7.2 7.3 7.4 7.5 7.6 7.7 Shaw (2008), p. 6-134.
  8. ↑ 8.0 8.1 Shaw (2008), p. 6-129.
  9. ↑ 9.0 9.1 Shaw (2008), p. 6-137.
  10. ↑ Hirschler (2008b), p. 18-27.
  11. ↑ Karlsson and Quintiere (1999a), as cited in Iqbal and Salley (2004), p. 2-22.
  12. ↑ 12.0 12.1 Budnick et al. (2008), p. 3-159.
  13. ↑ Quintiere (2002b), p. 2-251.
  14. ↑ SFPE Engineering Guide (2002), as cited in Iqbal and Salley (2004), p. 6-8.
  15. ↑ Iqbal and Salley (2004), p. 6-7.
  16. ↑ SFPE Engineering Guide (2002), as cited in Iqbal and Salley (2004), pp. 6-10–6-11.
  17. ↑ White (2002), p. 4-261.
  18. ↑ Corbett (2008), p. 12-131.
  19. ↑ Cholin (2008c), p. 6-66.
  20. ↑ Janssens (2002), p. 3-38.
  21. ↑ Babrauskas (2002a), p. 3-70.
  22. ↑ 22.0 22.1 22.2 Shaw (2008), p. 6-136.
  23. ↑ Gore Willse (2008b), p. 19-23.
  24. ↑ Shaw (2008), p. 6-138.
  25. ↑ Miller and Roether (2008), p. 20-89.
  26. ↑ Grill and Johnson (2005b), p. 53.
  27. ↑ Averill et al. (2005), p. 4.
  28. ↑ 28.0 28.1 Ministry of Business, Innovation and Employment (2013), p. 141.

References

  • Averill, J. D., Mileti, D. S., Peacock, R. D., Kuligowski, E. D., Groner, N., Proulx, G., Reneke, P. A., & Nelson, H. E. (2005). Occupant behavior, egress, and emergency communications (NIST NCSTAR 1-7). National Institute of Standards and Technology.
  • Babrauskas, V. (2002a). The cone calorimeter. In P. J. DiNenno, D. Drysdale, C. L. Beyler, W. D. Walton, R. L. P. Custer, J. R. Hall Jr., & J. M. Watts Jr. (Eds.), SFPE handbook of fire protection engineering (3rd ed., pp. 3-63–3-81). National Fire Protection Association; Society of Fire Protection Engineers.
  • Budnick, E. K., Hunt, S. P., & Wright, M. T. (2008). Closed form enclosure fire calculations. In A. E. Cote, C. C. Grant, J. R. Hall Jr., & R. E. Solomon (Eds.), Fire protection handbook (20th ed., pp. 3-145–3-166). National Fire Protection Association.
  • Cholin, J. M. (2008c). Wood and wood-based products. In A. E. Cote, C. C. Grant, J. R. Hall Jr., & R. E. Solomon (Eds.), Fire protection handbook (20th ed., pp. 6-61–6-74). National Fire Protection Association.
  • Corbett, G. P. (2008). Effect of building construction and fire protection systems on fire fighter safety. In A. E. Cote, C. C. Grant, J. R. Hall Jr., & R. E. Solomon (Eds.), Fire protection handbook (20th ed., pp. 12-127–12-141). National Fire Protection Association.
  • Gore Willse, P. J. (2008b). Types of building construction. In A. E. Cote, C. C. Grant, J. R. Hall Jr., & R. E. Solomon (Eds.), Fire protection handbook (20th ed., pp. 19-3–19-27). National Fire Protection Association.
  • Grill, R. A., & Johnson, D. A. (2005b). Fire protection and life safety provisions applied to the design and construction of WTC 1, 2, and 7 and post-construction provisions applied after occupancy (NIST NCSTAR 1-1D). National Institute of Standards and Technology.
  • Hirschler, M. M. (2008b). Interior finish. In A. E. Cote, C. C. Grant, J. R. Hall Jr., & R. E. Solomon (Eds.), Fire protection handbook (20th ed., pp. 18-23–18-42). National Fire Protection Association.
  • Iqbal, N., & Salley, M. H. (2004). Fire Dynamics Tools (FDTs): Quantitative fire hazard analysis methods for the U.S. Nuclear Regulatory Commission Fire Protection Inspection Program (NUREG-1805). U.S. Nuclear Regulatory Commission, Office of Nuclear Reactor Regulation.
  • Janssens, M. (2002). Calorimetry. In P. J. DiNenno, D. Drysdale, C. L. Beyler, W. D. Walton, R. L. P. Custer, J. R. Hall Jr., & J. M. Watts Jr. (Eds.), SFPE handbook of fire protection engineering (3rd ed., pp. 3-38–3-62). National Fire Protection Association; Society of Fire Protection Engineers.
  • Miller, G., & Roether, E. (2008). Assembly occupancies. In A. E. Cote, C. C. Grant, J. R. Hall Jr., & R. E. Solomon (Eds.), Fire protection handbook (20th ed., pp. 20-85–20-95). National Fire Protection Association.
  • Ministry of Business, Innovation and Employment. (2013). Commentary for Building Code clauses C1–C6 and Verification Method C/VM2.
  • Quintiere, J. G. (2002b). Surface flame spread. In P. J. DiNenno, D. Drysdale, C. L. Beyler, W. D. Walton, R. L. P. Custer, J. R. Hall Jr., & J. M. Watts Jr. (Eds.), SFPE handbook of fire protection engineering (3rd ed., pp. 2-246–2-257). National Fire Protection Association; Society of Fire Protection Engineers.
  • Shaw, J. R. (2008). Fire-Retardant and flame-resistant treatment of cellulosic materials. In A. E. Cote, C. C. Grant, J. R. Hall Jr., & R. E. Solomon (Eds.), Fire protection handbook (20th ed., pp. 6-129–6-139). National Fire Protection Association.
  • White, R. H. (2002). Analytical methods for determining fire resistance of timber members. In P. J. DiNenno, D. Drysdale, C. L. Beyler, W. D. Walton, R. L. P. Custer, J. R. Hall Jr., & J. M. Watts Jr. (Eds.), SFPE handbook of fire protection engineering (3rd ed., pp. 4-257–4-273). National Fire Protection Association; Society of Fire Protection Engineers.