Skip to content
From Fire Safety Academy Wiki
Revision as of 22:27, 7 November 2026 by Jan (talk | contribs) (NFPA wiki: fact-check corrections (written by Claude Opus 5.5))
Contents
  1. 1Definition and scope
  2. 2Thermoplastics, thermosets and feedstock
  3. 3Main processes
  4. 4Fire and explosion hazards
    1. 4.1Combustible dust
    2. 4.2Flammable solvents and blowing agents
    3. 4.3Heaters and decomposition
    4. 4.4Static electricity
    5. 4.5Hydraulic and heat transfer fluids
    6. 4.6Storage of raw material and product
  5. 5Fire load and a worked example
  6. 6Typical values
  7. 7Safeguards
  8. 8Limits of the sources
  9. 9See also
  10. 10Notes
  11. 11References

Plastics processing is the conversion of plastic feedstock into finished articles. The material is heated until it flows, shaped in a mould or die, and cooled or cured so that the shape is kept. Moulding, extrusion, foaming and casting are the main techniques.[1] In a wider sense the plastics industry also covers synthesis of the polymer, compounding and mechanical fabrication, and each stage has its own fire hazards.[2] A processing plant combines several hazards in one building. The Fire Protection Handbook (2008), describing United States practice, names combustible dust, flammable liquids, high-heat elements, static electricity, hydraulic and heat transfer fluids, and poor storage and housekeeping.[3] Most plastics are combustible organic compounds,[1] and many burn like flammable liquids once they melt or break down in a fire.[4] The fire behaviour of the finished materials is treated in Plastics in fire.

Definition and scope

The handbook chapter on the plastics industry defines processing as "the converting of polymers into useful articles by molding or extrusion from granules, depositing film from solvent, or laminating resin and reinforcement". It adds that the moulding step most often uses heat but is largely or entirely a physical rather than a chemical process.[5] The handbook also prints the ASTM definition of a plastic. It is a material with one or more organic polymers of large molecular weight as an essential ingredient. It is solid in its finished state and can be shaped by flow at some stage of manufacture or processing.[6] Plastics are built from small "mer" units, or monomers, which polymerisation links into long chains of high molecular weight.[7]

The handbook divides the industry into four broad areas: polymerisation or synthesis, manufacturing, conversion and fabrication. They can take place at one site or at different sites, and each has its own types and levels of hazard.[2] In polymerisation the monomer reacts with catalysts and gases in a reactor. The result is the basic polymer as a powder, granules or a viscous liquid. Polyethylene shows how the product changes as the chain grows. Ethylene is a gas with a molecular weight of 28; six mer units give a liquid, 35 a grease and 140 a wax. At 430 mer units the product is a hard resin with a molecular weight of 12,000.[2]

In manufacturing the polymer is put into a form that is easy to handle. The most common process is compounding with colourants, rubber, fillers, reinforcements, flame retardants and other additives.[1]

Conversion is the step the industry itself calls "processing" or "converting". It usually involves heating the plastic so that it flows into a shape that is kept on cooling. Thermoplastics normally undergo no chemical reaction here. For thermosetting resins, the cross-linking reaction that fixes the final shape is a significant part of the operation. Fabrication covers the largely mechanical operations of bending, machining, cementing, welding, heat sealing, decorating and polishing.[1]

The distinction matters for fire safety. The synthesis of a given plastic may be much more hazardous than its moulding or extrusion. Yet some plants that only convert or fabricate also run chemical operations with flammable or reactive materials. The handbook's example is the moulding of boat hulls from glass fibres impregnated with liquid polyester resin.[1] The polymerisation step is described as the most hazardous, because of the large amounts of gases and flammable liquids involved.[1]

Thermoplastics, thermosets and feedstock

Every plastic belongs to one of two groups, explained in more detail in Thermoplastics and thermosets. A thermoplastic can be softened by heating and hardened by cooling many times without a major chemical change. Reprocessing can still break some chains and lower the molecular weight and viscosity. A thermoset undergoes a chemical reaction when heat treated. Afterwards it cannot be softened without a significant chemical change.[7][2]

The SFPE Handbook describes the same split in terms of deformation. For thermoplastics the deformation at elevated temperature is reversible, while thermosets undergo irreversible changes when heated.[8] Thermosets have a rigid cross-linked molecular structure. Thermoplastics have a more flexible structure, with side chains that are not rigidly linked to other molecules.[6]

Many feedstocks are derived from petroleum or natural gas. Ethylene monomer, for example, comes in gaseous form from refinery gas, liquefied petroleum gas or liquid hydrocarbons.[9] The resin usually reaches the processor as pellets, granules, flakes or powder. Some feedstocks come as pastes or as liquids for casting.[9] Thermoplastic feedstock is melted by heat, pressure forces the melt into a mould cavity or through a die, and cooling lets it harden. With thermosets, heat and pressure are also used, but the heat triggers the curing reaction in the mould.[9]

Main processes

Extrusion passes molten plastic under pressure through a die to form a continuous profile; the machine is called an extruder.[1] It makes sheeting, film, tubes, rods, profiles and filaments, and it coats wire and cable. In a single-screw extruder, pellets or powder fall from a hopper through the feed throat onto a screw. The screw turns in a heated barrel, melts the plastic and pushes it through a breaker plate and an adapter into the die.[10][11] Screw extruders have largely displaced rolls and kneaders for compounding. They give better control, continuous output and less exposure of hot plastic to air. The extrudate is normally cooled in a water bath and chopped into pellets.[10]

Injection moulding forms objects from pelletised, granular or powdered plastic, most often thermoplastic. The material is softened in a heated chamber, and a ram or screw forces it into a mould. Pressure is held until the part is hard enough to remove.[11] In the common reciprocating-screw machine, the screw first melts a shot of plastic in front of its tip. A hydraulic injection cylinder then pushes the screw forward like a plunger.[11] Blow moulding is used almost only with thermoplastics, for hollow articles such as bottles and car fuel tanks. A molten tube, the parison, is sealed, placed in a mould and inflated with air against the mould walls.[9]

Calendering passes the softened compound between three or four large heated rolls that turn at different speeds.[10] Compression moulding, the most common method for thermosets, squeezes material into shape in a heated mould.[10] Transfer moulding is similar, but a plunger forces the material from a pot into a closed mould.[3] Reaction injection moulding, used mainly for polyurethane, impinges two or more reactive streams under high pressure in a mixing chamber and injects the mixture under low pressure into a mould, where it reacts.[12] Rotational moulding turns a heated mould about two axes to make hollow parts such as barrels. Thermoforming presses heated sheet against a mould mechanically, by vacuum or by compressed air.[12]

Foam products need a blowing agent, which produces gas by thermal or chemical action and expands the plastic into a cellular structure.[1] In steam-chest moulding, expandable polystyrene beads that contain a blowing agent are pre-expanded with steam. They are then dried in a hopper and fused in the final mould with more steam.[11] Laminating uses thermosetting resins to bind cloth, paper, wood or glass fibre. The handbook separates high-pressure laminating, at 200 psi or more, from low-pressure laminating below that value. It prints the conversion as "1.4 kPa", but 200 psi is about 1.4 MPa.[11][12]

Fire and explosion hazards

The hazards specific to converting plants come on top of those common to most industrial operations.[3] The handbook groups them as dust, flammable liquids, heaters, static electricity, hydraulic and heat transfer fluids, and storage.

Combustible dust

Many plastics in solid form are difficult to ignite and stop burning when an exposing flame is removed. Nearly all of them burn rapidly as dust, however. A dust cloud in air can be ignited explosively by a spark, a flame or a surface hotter than the flash ignition temperature of the material.[3] A Dust explosion should therefore be considered where pulverised plastic is used, granules are conveyed pneumatically, or machining or sanding produces dust.[3] Moulding pellets are cubes or cylinders, usually screened to remove fines, and are free from the dust explosion hazard. Fines can still form by abrasion in long pneumatic conveying lines, and regrinding of runners, sprues and flash usually makes some fine powder.[3]

Compounding is another source, because additives are charged to mixers as fine powders. Wood flour, cotton flock and other combustible fillers usually increase the explosibility of a dust. Low percentages of fire retardants have little effect.[3] Test data show how severe plastic dust explosions can be. The deflagration index KSt is the maximum rate of pressure rise in a closed test vessel multiplied by the cube root of the vessel volume.[13] Pmax is the maximum explosion pressure. For low-density polyethylene with a median particle size below 10 µm, the SFPE Handbook lists a KSt of 156 bar·m/s. For 150 µm particles the value is 54 bar·m/s, so the fine dust is almost three times as severe.[14] The minimum explosible concentration is 30 g/m³ for the fine dust, measured in a 1.2 litre cylinder, and 125 g/m³ for the coarse one, measured in a 1 m³ vessel.[14]

Flammable solvents and blowing agents

Flammable organic solvents are found in nearly every plastics plant. Small amounts serve for adhesives, lacquers, paints and cleaning. Large amounts are used to coat plastic onto cloth, paper, leather or metal.[3] Solvent foaming is a further source. The most common rigid foam is made from polystyrene beads moistened with about 10 percent pentane or a similar hydrocarbon. The pentane expands the resin at the temperature of low-pressure steam.[15] Containers of such resin hold free pentane vapour and should be opened outdoors or under good exhaust ventilation. Expanded articles should be aged under forced hot air before shipping, to drive off nearly all of the blowing agent.[15]

Chemical blowing agents behave differently. Azodicarbonamide, used for expanded vinyl, gives off nitrogen above 300 °F (149 °C) and no flammable vapour.[15] According to the handbook, the most frequent cause of flammable-liquid fires in plastics plants has been a failure to deal with three things. These are electrostatic sparks, the need for explosion-proof electrical equipment, and vapour removal.[15]

Heaters and decomposition

Moulding and extrusion machines run at about 300 to 650 °F (149 to 343 °C), depending on the plastic. The upper part of that range is beyond what is practical for a Heat transfer fluid system. Electric resistance heater bands are therefore almost universally used on barrels.[15] Temperature controllers can stick and let the heaters exceed their set point. In most cases the extrudate changes visibly and warns the operator before the bands become hot enough to ignite anything.[15]

Material trapped in areas that the feedstock does not purge can be kept too hot or too long. It may then decompose and release gases that can be combustible. The handbook advises heating such equipment from the downstream end first, so that pressure can escape. It also warns against standing in front of an extruder while it heats up.[15] Ignition data help to judge the margin. For thermoplastics as a group, piloted ignition temperatures of 369 ± 73 °C and autoignition temperatures of 457 ± 63 °C are reported. For thermosetting plastics the values are 441 ± 100 °C and 514 ± 92 °C.[16]

Static electricity

Friction, heat and pressure in plastics operations generate Static electricity. Because plastics are good insulators, the charge can quickly build up to a spark discharge. This is hazardous where dust or flammable vapour is present.[15] Typical sources are stripping films from equipment, fast passage of film over rolls and guides, and power transmission belts. High humidity, used in cotton, wool and paper mills, does not dissipate the charge on plastics. Their low water absorption and high resistivity prevent it.[15]

The handbook names three ways to neutralise the charge: induction, grounding and ionisation. Tinsel is the most common induction method. It needs a conductive metal core, must be grounded and stretched tight, and should run ¼ in. (6 mm) from the material. It never reduces the charge to zero.[15]

Hydraulic and heat transfer fluids

Hydraulic systems clamp the moulds and drive the rams and screws of moulding machines. The molten plastic can reach 30,000 psi (207 MPa), but the hydraulic systems normally work below 2000 psi (13.8 MPa).[15][4] Petroleum hydraulic oils have been used where heating elements stay below about 600 °F (315 °C). The same oils have a poor fire record in die casting of metals. There the molten metal is far hotter than the ignition temperature of the fluid.[4] Fire-resistant water-glycol fluids, water-oil emulsions and synthetic fluids are available. A change of fluid should follow the advice of the makers of the hydraulic components.[4]

The handbook chapter on fluid power lists plastic moulding among operations with constantly present ignition sources. Pressurised petroleum oils are a considerable fire hazard there.[17] A failed hose or fitting usually releases an atomised spray of oil droplets. The spray ignites readily and gives a torch-like Jet fire with a very high rate of heat release.[18] Rolls and kneaders used for compounding are heated with high-pressure steam or with heat transfer fluids.[10]

Storage of raw material and product

The fire hazard of stored plastics depends on their chemical composition, physical form and storage arrangement. A fire usually produces large quantities of smoke and toxic gases such as carbon monoxide, which makes manual fire fighting difficult.[4] Several common plastics can melt or depolymerise into fractions that act and burn like flammable liquids. The handbook names polystyrene, ABS (acrylonitrile-butadiene-styrene), polyurethane, polyethylene, polypropylene, plasticised PVC (polyvinyl chloride) and polyesters.[4] In foamed form these plastics present the most severe hazard, because they ignite more easily and burn faster; Foam plastic insulation is one such product.[4][5] Some unstabilised polymer powders decompose slowly in storage. If the heat is not lost, the temperature can rise until self-accelerating decomposition is reached, so container temperatures should be monitored.[4]

Fire load and a worked example

The International Fire Engineering Guidelines (2005) reproduce fire load densities from Swiss surveys of 1967–1969. Values for manufacturing are given per square metre of floor. Values for storage are given per square metre and per metre of storage height, and must be multiplied by the height of the goods.[19] "Plastic processing" and "Plastic products fabrication" are both listed at 600 MJ/m². "Injection moulded parts mfg (plastic)" is listed at 500 MJ/m² and "Foamed plastics fabrication" at 3000 MJ/m².[20][21] "Plastic mfg" has 2000 MJ/m² for manufacturing and 5900 MJ/m² per metre of height for storage.[21]

The total fire load of an area is the fire load density times the floor area. For storage, the density per metre of height is first multiplied by the storage height: Q=qfAandqf,storage=qsh

Symbol Description Unit
Q total fire load of the area MJ
qf fire load density per unit floor area MJ/m²
A floor area m²
qs storage fire load density per unit floor area and per metre of storage height MJ/m² per m
h storage height m

As a worked example, take a processing hall of 2000 m² with the tabulated average of 600 MJ/m². It holds about 1.2 TJ of fire load. For industrial occupancies the guidelines tentatively suggest a 90 % fractile of 1.65 to 2.0 times the average. That gives 990 to 1200 MJ/m²; taking the upper value is the conservative choice.[19] Now take an adjoining store of plastic material stacked 3 m high, with the "Plastic mfg" storage value. It reaches 5900 × 3 = 17,700 MJ/m², about 30 times the density of the processing floor. The handbook separately advises separating storage and manufacturing areas by fire-rated walls.[22] The values are averages from one country and period. The guidelines warn that fire loads have changed with new technologies and materials.[19]

Typical values

The table collects values from the sources for processing conditions and common plastics. Dust data depend strongly on particle size and test method. They describe the tested samples only.

Quantity Value Conditions Source
Barrel operating temperature, moulding and extrusion 149–343 °C (300–650 °F) depends on plastic [15]
Melt pressure in moulding up to 207 MPa (30,000 psi) compression, transfer, injection moulding [4]
Hydraulic system pressure normally below 13.8 MPa (2000 psi) mould clamps, rams, screws [4]
KSt, polyethylene (low density) 156 bar·m/s; 54 bar·m/s median size below 10 µm; 150 µm [14]
Pmax, polyethylene (low density) 8.0 bar g; 7.4 bar g median size below 10 µm; 150 µm [14]
Cloud ignition temperature, PVC dust 750 °C median size 25 µm [14]
KSt, ABS dust 147 bar·m/s particle size 200 µm, 1 m³ or 20 litre vessel [23][24]
KSt, polypropylene dust 101 bar·m/s particle size 25 µm, 1 m³ or 20 litre vessel [23]
KSt, polystyrene hard foam dust 23 bar·m/s particle size 760 µm, 1 m³ or 20 litre vessel [23]
Pentane in expandable polystyrene beads about 10 percent rigid foam feedstock [15]
Fire load density, plastic processing 600 MJ/m² Swiss surveys 1967–1969 [21]

Safeguards

The handbook states that fire protection starts with fire-safe design of the plant or warehouse. It considers sprinkler-protected, noncombustible construction appropriate for buildings that store, process or manufacture plastics.[4] It prefers one-storey buildings without basements, and long, narrow buildings to large square ones. Large properties should be divided into separate fire areas, with storage and manufacturing separated by fire-rated walls. In the United States practice it describes, a single fire area should generally not exceed 50,000 ft² (4645 m²).[22] Roof vents are to be considered, particularly in large one-storey warehouses.[4]

Sprinklers are described as the most important single system for automatic fire control in plastics plants. They operate directly over the fire and are not affected by smoke or poor visibility. Processing equipment, conveyors and machinery that can ignite or explode can carry fire, smoke or explosion detectors. These raise the alarm and release water spray, foam, dry chemical, carbon dioxide or halogenated agents.[22] For dust, the chapter points to NFPA 654 on combustible particulate solids. It also cites NFPA 68 on deflagration venting and NFPA 69 on explosion prevention systems, without stating their editions.[3] For flammable liquids and static it refers to NFPA 30, 33, 35, 70, 77 and 91.[15]

Housekeeping controls unwanted fuel and ignition sources. Dust and lint are removed from walls, ceilings and structural members, spills are cleaned up, and smoking is banned in process and storage areas.[4] Plastics are thermal insulators, so purged material from extruders and moulding machines can stay molten inside long after its surface has set. It must be put down in a safe place and should not go into rubbish containers until it has cooled completely.[4] Staff training covers the safety data sheets of every plastic, additive and solvent. It also covers the location of alarms, extinguishers and power switches. Simple actions, such as shutting off power or dumping the water of an extruder cooling bath onto smouldering plastic, can stop a small fire.[22]

Limits of the sources

The handbook chapter describes United States practice around 2007–2008. It refers to NFPA standards without their editions, so its recommendations describe that time and place, not current requirements. The chapter has at least two evident misprints: the conversion of 200 psi as "1.4 kPa", and the year 1962 for the first man-made plastic by Alexander Parkes.[7][12] The plastics dust table in the handbook is derived from data published by Eckhoff and, before that, by the German BIA. Its particle size column is printed with a damaged unit symbol.[23] The fire load densities come from Swiss surveys more than 50 years old.[19]

See also

Notes

  1. ↑ 1.0 1.1 1.2 1.3 1.4 1.5 1.6 1.7 Ouellette (2008), p. 9-55.
  2. ↑ 2.0 2.1 2.2 2.3 Ouellette (2008), p. 9-54.
  3. ↑ 3.0 3.1 3.2 3.3 3.4 3.5 3.6 3.7 3.8 Ouellette (2008), p. 9-61.
  4. ↑ 4.00 4.01 4.02 4.03 4.04 4.05 4.06 4.07 4.08 4.09 4.10 4.11 4.12 4.13 Ouellette (2008), p. 9-63.
  5. ↑ 5.0 5.1 Ouellette (2008), p. 9-56.
  6. ↑ 6.0 6.1 Benedetti and Colonna (2008), p. 6-210.
  7. ↑ 7.0 7.1 7.2 Ouellette (2008), p. 9-53.
  8. ↑ Beyler and Hirschler (2002), p. 1-111.
  9. ↑ 9.0 9.1 9.2 9.3 Ouellette (2008), p. 9-57.
  10. ↑ 10.0 10.1 10.2 10.3 10.4 Ouellette (2008), p. 9-58.
  11. ↑ 11.0 11.1 11.2 11.3 11.4 Ouellette (2008), p. 9-59.
  12. ↑ 12.0 12.1 12.2 12.3 Ouellette (2008), p. 9-60.
  13. ↑ Zalosh (2002), p. 3-409.
  14. ↑ 14.0 14.1 14.2 14.3 14.4 Zalosh (2002), p. 3-404.
  15. ↑ 15.00 15.01 15.02 15.03 15.04 15.05 15.06 15.07 15.08 15.09 15.10 15.11 15.12 15.13 Ouellette (2008), p. 9-62.
  16. ↑ Babrauskas (2003), as cited in National Research Council of Canada et al. (2005), p. 3.3-4.
  17. ↑ Schacht (2008), p. 8-113.
  18. ↑ Schacht (2008), p. 8-114.
  19. ↑ 19.0 19.1 19.2 19.3 National Research Council of Canada et al. (2005), p. 3.4-2.
  20. ↑ National Research Council of Canada et al. (2005), p. 3.4-5.
  21. ↑ 21.0 21.1 21.2 National Research Council of Canada et al. (2005), p. 3.4-6.
  22. ↑ 22.0 22.1 22.2 22.3 Ouellette (2008), p. 9-64.
  23. ↑ 23.0 23.1 23.2 23.3 Schwab (2008c), p. 6-146.
  24. ↑ Schwab (2008c), p. 6-147.

References

  • Benedetti, R. P., & Colonna, G. R. (2008). Polymeric materials. In A. E. Cote, C. C. Grant, J. R. Hall Jr., & R. E. Solomon (Eds.), Fire protection handbook (20th ed., pp. 6-209–6-231). National Fire Protection Association.
  • Beyler, C. L., & Hirschler, M. M. (2002). Thermal decomposition of polymers. In P. J. DiNenno, D. Drysdale, C. L. Beyler, W. D. Walton, R. L. P. Custer, J. R. Hall Jr., & J. M. Watts Jr. (Eds.), SFPE handbook of fire protection engineering (3rd ed., pp. 1-110–1-131). National Fire Protection Association; Society of Fire Protection Engineers.
  • National Research Council of Canada, International Code Council, Department of Building and Housing, & Australian Building Codes Board. (2005). International fire engineering guidelines (2005 ed.). Australian Building Codes Board.
  • Ouellette, G. (2008). Plastics industry and related process hazards. In A. E. Cote, C. C. Grant, J. R. Hall Jr., & R. E. Solomon (Eds.), Fire protection handbook (20th ed., pp. 9-53–9-65). National Fire Protection Association.
  • Schacht, P. K. (2008). Fluid power systems. In A. E. Cote, C. C. Grant, J. R. Hall Jr., & R. E. Solomon (Eds.), Fire protection handbook (20th ed., pp. 8-113–8-116). National Fire Protection Association.
  • Schwab, R. F. (2008c). Dusts. In A. E. Cote, C. C. Grant, J. R. Hall Jr., & R. E. Solomon (Eds.), Fire protection handbook (20th ed., pp. 6-141–6-152). National Fire Protection Association.
  • Zalosh, R. (2002). Explosion protection. In P. J. DiNenno, D. Drysdale, C. L. Beyler, W. D. Walton, R. L. P. Custer, J. R. Hall Jr., & J. M. Watts Jr. (Eds.), SFPE handbook of fire protection engineering (3rd ed., pp. 3-402–3-421). National Fire Protection Association; Society of Fire Protection Engineers.