<?xml version="1.0"?>
<feed xmlns="http://www.w3.org/2005/Atom" xml:lang="en">
	<id>https://fire-safety.academy/w/index.php?action=history&amp;feed=atom&amp;title=Prestressed_concrete_in_fire</id>
	<title>Prestressed concrete in fire - Revision history</title>
	<link rel="self" type="application/atom+xml" href="https://fire-safety.academy/w/index.php?action=history&amp;feed=atom&amp;title=Prestressed_concrete_in_fire"/>
	<link rel="alternate" type="text/html" href="https://fire-safety.academy/w/index.php?title=Prestressed_concrete_in_fire&amp;action=history"/>
	<updated>2026-11-21T23:34:29Z</updated>
	<subtitle>Revision history for this page on the wiki</subtitle>
	<generator>MediaWiki 1.43.11</generator>
	<entry>
		<id>https://fire-safety.academy/w/index.php?title=Prestressed_concrete_in_fire&amp;diff=9481&amp;oldid=prev</id>
		<title>Peter: Wiki review: corrected 4 errors: typo (3), markup (Claude Opus 5.5)</title>
		<link rel="alternate" type="text/html" href="https://fire-safety.academy/w/index.php?title=Prestressed_concrete_in_fire&amp;diff=9481&amp;oldid=prev"/>
		<updated>2026-11-15T23:50:52Z</updated>

		<summary type="html">&lt;p&gt;Wiki review: corrected 4 errors: typo (3), markup (Claude Opus 5.5)&lt;/p&gt;
&lt;table style=&quot;background-color: #fff; color: #202122;&quot; data-mw=&quot;interface&quot;&gt;
				&lt;col class=&quot;diff-marker&quot; /&gt;
				&lt;col class=&quot;diff-content&quot; /&gt;
				&lt;col class=&quot;diff-marker&quot; /&gt;
				&lt;col class=&quot;diff-content&quot; /&gt;
				&lt;tr class=&quot;diff-title&quot; lang=&quot;en&quot;&gt;
				&lt;td colspan=&quot;2&quot; style=&quot;background-color: #fff; color: #202122; text-align: center;&quot;&gt;← Older revision&lt;/td&gt;
				&lt;td colspan=&quot;2&quot; style=&quot;background-color: #fff; color: #202122; text-align: center;&quot;&gt;Revision as of 00:50, 16 November 2026&lt;/td&gt;
				&lt;/tr&gt;&lt;tr&gt;&lt;td colspan=&quot;2&quot; class=&quot;diff-lineno&quot; id=&quot;mw-diff-left-l8&quot;&gt;Line 8:&lt;/td&gt;
&lt;td colspan=&quot;2&quot; class=&quot;diff-lineno&quot;&gt;Line 8:&lt;/td&gt;&lt;/tr&gt;
&lt;tr&gt;&lt;td class=&quot;diff-marker&quot;&gt;&lt;/td&gt;&lt;td style=&quot;background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;&quot;&gt;&lt;br&gt;&lt;/td&gt;&lt;td class=&quot;diff-marker&quot;&gt;&lt;/td&gt;&lt;td style=&quot;background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;&quot;&gt;&lt;br&gt;&lt;/td&gt;&lt;/tr&gt;
&lt;tr&gt;&lt;td class=&quot;diff-marker&quot;&gt;&lt;/td&gt;&lt;td style=&quot;background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;&quot;&gt;&lt;div&gt;Prestressing introduces forces before the member carries its full service loading; the NFPA handbook explains that the steel therefore begins fire exposure under substantial initial stress. Heating changes its strength, stiffness and time-dependent deformation. These effects can reduce the prestressing force and the capacity of the complete member.&amp;lt;ref name=&amp;quot;NFPA-§19.2,p.19-53&amp;quot;&amp;gt;Cote et al. (2008), §19.2, p. 19-53.&amp;lt;/ref&amp;gt;&lt;/div&gt;&lt;/td&gt;&lt;td class=&quot;diff-marker&quot;&gt;&lt;/td&gt;&lt;td style=&quot;background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;&quot;&gt;&lt;div&gt;Prestressing introduces forces before the member carries its full service loading; the NFPA handbook explains that the steel therefore begins fire exposure under substantial initial stress. Heating changes its strength, stiffness and time-dependent deformation. These effects can reduce the prestressing force and the capacity of the complete member.&amp;lt;ref name=&amp;quot;NFPA-§19.2,p.19-53&amp;quot;&amp;gt;Cote et al. (2008), §19.2, p. 19-53.&amp;lt;/ref&amp;gt;&lt;/div&gt;&lt;/td&gt;&lt;/tr&gt;
&lt;tr&gt;&lt;td class=&quot;diff-marker&quot; data-marker=&quot;−&quot;&gt;&lt;/td&gt;&lt;td style=&quot;color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #ffe49c; vertical-align: top; white-space: pre-wrap;&quot;&gt;&lt;div&gt;[[File:fse-prestressed-concrete-in-fire-v1.svg|thumb|upright=1.5|alt=Prestressed concrete in fire: prestress, heating and the resisting system, showing the relationships described in the text.|Prestress, heating and the resisting system in the assessment of &lt;del style=&quot;font-weight: bold; text-decoration: none;&quot;&gt;Prestressed &lt;/del&gt;concrete in fire.]]&lt;/div&gt;&lt;/td&gt;&lt;td class=&quot;diff-marker&quot; data-marker=&quot;+&quot;&gt;&lt;/td&gt;&lt;td style=&quot;color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #a3d3ff; vertical-align: top; white-space: pre-wrap;&quot;&gt;&lt;div&gt;[[File:fse-prestressed-concrete-in-fire-v1.svg|thumb|upright=1.5|alt=Prestressed concrete in fire: prestress, heating and the resisting system, showing the relationships described in the text.|Prestress, heating and the resisting system in the assessment of &lt;ins style=&quot;font-weight: bold; text-decoration: none;&quot;&gt;prestressed &lt;/ins&gt;concrete in fire.]]&lt;/div&gt;&lt;/td&gt;&lt;/tr&gt;
&lt;tr&gt;&lt;td class=&quot;diff-marker&quot;&gt;&lt;/td&gt;&lt;td style=&quot;background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;&quot;&gt;&lt;br&gt;&lt;/td&gt;&lt;td class=&quot;diff-marker&quot;&gt;&lt;/td&gt;&lt;td style=&quot;background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;&quot;&gt;&lt;br&gt;&lt;/td&gt;&lt;/tr&gt;
&lt;tr&gt;&lt;td class=&quot;diff-marker&quot;&gt;&lt;/td&gt;&lt;td style=&quot;background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;&quot;&gt;&lt;div&gt;The distinction from ordinary reinforced concrete is not simply a different concrete strength. The function and type of steel matter, as do the initial force and its transfer into the concrete. [[Strength reduction at elevated temperatures]] must therefore be represented for the actual tendon material. A relationship for ordinary hot-rolled reinforcement does not establish every prestressing-steel response.&amp;lt;ref name=&amp;quot;NFPA-§19.2,pp.19-53-19-54&amp;quot; /&amp;gt;&lt;/div&gt;&lt;/td&gt;&lt;td class=&quot;diff-marker&quot;&gt;&lt;/td&gt;&lt;td style=&quot;background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;&quot;&gt;&lt;div&gt;The distinction from ordinary reinforced concrete is not simply a different concrete strength. The function and type of steel matter, as do the initial force and its transfer into the concrete. [[Strength reduction at elevated temperatures]] must therefore be represented for the actual tendon material. A relationship for ordinary hot-rolled reinforcement does not establish every prestressing-steel response.&amp;lt;ref name=&amp;quot;NFPA-§19.2,pp.19-53-19-54&amp;quot; /&amp;gt;&lt;/div&gt;&lt;/td&gt;&lt;/tr&gt;
&lt;tr&gt;&lt;td colspan=&quot;2&quot; class=&quot;diff-lineno&quot; id=&quot;mw-diff-left-l19&quot;&gt;Line 19:&lt;/td&gt;
&lt;td colspan=&quot;2&quot; class=&quot;diff-lineno&quot;&gt;Line 19:&lt;/td&gt;&lt;/tr&gt;
&lt;tr&gt;&lt;td class=&quot;diff-marker&quot;&gt;&lt;/td&gt;&lt;td style=&quot;background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;&quot;&gt;&lt;br&gt;&lt;/td&gt;&lt;td class=&quot;diff-marker&quot;&gt;&lt;/td&gt;&lt;td style=&quot;background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;&quot;&gt;&lt;br&gt;&lt;/td&gt;&lt;/tr&gt;
&lt;tr&gt;&lt;td class=&quot;diff-marker&quot;&gt;&lt;/td&gt;&lt;td style=&quot;background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;&quot;&gt;&lt;div&gt;Cover is part of the thermal protection around the steel. Its effectiveness depends on remaining in place and on the distance from the exposed face to the tendon. The NFPA handbook notes that spalling can expose prestressing steel directly. The member then has both a changed cross-section and a changed heating boundary.&amp;lt;ref name=&amp;quot;NFPA-§19.2,pp.19-53-19-54&amp;quot; /&amp;gt;&lt;/div&gt;&lt;/td&gt;&lt;td class=&quot;diff-marker&quot;&gt;&lt;/td&gt;&lt;td style=&quot;background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;&quot;&gt;&lt;div&gt;Cover is part of the thermal protection around the steel. Its effectiveness depends on remaining in place and on the distance from the exposed face to the tendon. The NFPA handbook notes that spalling can expose prestressing steel directly. The member then has both a changed cross-section and a changed heating boundary.&amp;lt;ref name=&amp;quot;NFPA-§19.2,pp.19-53-19-54&amp;quot; /&amp;gt;&lt;/div&gt;&lt;/td&gt;&lt;/tr&gt;
&lt;tr&gt;&lt;td class=&quot;diff-marker&quot; data-marker=&quot;−&quot;&gt;&lt;/td&gt;&lt;td style=&quot;color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #ffe49c; vertical-align: top; white-space: pre-wrap;&quot;&gt;&lt;div&gt;[[File:fse-prestressed-concrete-in-fire-v2.svg|thumb|upright=1.5|alt=Prestressed concrete in fire: cover, connections and the condition after cooling, showing the relationships described in the text.|Cover, connections and the condition after cooling in the assessment of &lt;del style=&quot;font-weight: bold; text-decoration: none;&quot;&gt;Prestressed &lt;/del&gt;concrete in fire.]]&lt;/div&gt;&lt;/td&gt;&lt;td class=&quot;diff-marker&quot; data-marker=&quot;+&quot;&gt;&lt;/td&gt;&lt;td style=&quot;color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #a3d3ff; vertical-align: top; white-space: pre-wrap;&quot;&gt;&lt;div&gt;[[File:fse-prestressed-concrete-in-fire-v2.svg|thumb|upright=1.5|alt=Prestressed concrete in fire: cover, connections and the condition after cooling, showing the relationships described in the text.|Cover, connections and the condition after cooling in the assessment of &lt;ins style=&quot;font-weight: bold; text-decoration: none;&quot;&gt;prestressed &lt;/ins&gt;concrete in fire.]]&lt;/div&gt;&lt;/td&gt;&lt;/tr&gt;
&lt;tr&gt;&lt;td class=&quot;diff-marker&quot;&gt;&lt;/td&gt;&lt;td style=&quot;background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;&quot;&gt;&lt;br&gt;&lt;/td&gt;&lt;td class=&quot;diff-marker&quot;&gt;&lt;/td&gt;&lt;td style=&quot;background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;&quot;&gt;&lt;br&gt;&lt;/td&gt;&lt;/tr&gt;
&lt;tr&gt;&lt;td class=&quot;diff-marker&quot;&gt;&lt;/td&gt;&lt;td style=&quot;background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;&quot;&gt;&lt;div&gt;A floor or roof is also a system of members and supports. Precast elements, bearings and connections have different dependencies from a continuous cast-in-place arrangement. The handbook&amp;#039;s firefighting discussion explains that roof loss can remove restraint from heavy wall panels. The structural consequences can extend beyond the heated concrete element.&amp;lt;ref name=&amp;quot;NFPA-§12.8,p.12-136&amp;quot;&amp;gt;Cote et al. (2008), §12.8, p. 12-136.&amp;lt;/ref&amp;gt;&lt;/div&gt;&lt;/td&gt;&lt;td class=&quot;diff-marker&quot;&gt;&lt;/td&gt;&lt;td style=&quot;background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;&quot;&gt;&lt;div&gt;A floor or roof is also a system of members and supports. Precast elements, bearings and connections have different dependencies from a continuous cast-in-place arrangement. The handbook&amp;#039;s firefighting discussion explains that roof loss can remove restraint from heavy wall panels. The structural consequences can extend beyond the heated concrete element.&amp;lt;ref name=&amp;quot;NFPA-§12.8,p.12-136&amp;quot;&amp;gt;Cote et al. (2008), §12.8, p. 12-136.&amp;lt;/ref&amp;gt;&lt;/div&gt;&lt;/td&gt;&lt;/tr&gt;
&lt;tr&gt;&lt;td colspan=&quot;2&quot; class=&quot;diff-lineno&quot; id=&quot;mw-diff-left-l108&quot;&gt;Line 108:&lt;/td&gt;
&lt;td colspan=&quot;2&quot; class=&quot;diff-lineno&quot;&gt;Line 108:&lt;/td&gt;&lt;/tr&gt;
&lt;tr&gt;&lt;td class=&quot;diff-marker&quot;&gt;&lt;/td&gt;&lt;td style=&quot;background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;&quot;&gt;&lt;br&gt;&lt;/td&gt;&lt;td class=&quot;diff-marker&quot;&gt;&lt;/td&gt;&lt;td style=&quot;background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;&quot;&gt;&lt;br&gt;&lt;/td&gt;&lt;/tr&gt;
&lt;tr&gt;&lt;td class=&quot;diff-marker&quot;&gt;&lt;/td&gt;&lt;td style=&quot;background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;&quot;&gt;&lt;div&gt;Fire resistance is evaluated against specified functions under a defined exposure. A separating concrete floor may need to support loads and limit heat transfer to the space above; a column has a different structural role and exposure arrangement. The required endpoints follow the assembly and assessment method, rather than the material name alone.&amp;lt;ref name=&amp;quot;concreteinfi_FB_4-239&amp;quot; /&amp;gt;&amp;lt;ref name=&amp;quot;concreteinfi_FB_4-242&amp;quot; /&amp;gt;&lt;/div&gt;&lt;/td&gt;&lt;td class=&quot;diff-marker&quot;&gt;&lt;/td&gt;&lt;td style=&quot;background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;&quot;&gt;&lt;div&gt;Fire resistance is evaluated against specified functions under a defined exposure. A separating concrete floor may need to support loads and limit heat transfer to the space above; a column has a different structural role and exposure arrangement. The required endpoints follow the assembly and assessment method, rather than the material name alone.&amp;lt;ref name=&amp;quot;concreteinfi_FB_4-239&amp;quot; /&amp;gt;&amp;lt;ref name=&amp;quot;concreteinfi_FB_4-242&amp;quot; /&amp;gt;&lt;/div&gt;&lt;/td&gt;&lt;/tr&gt;
&lt;tr&gt;&lt;td class=&quot;diff-marker&quot; data-marker=&quot;−&quot;&gt;&lt;/td&gt;&lt;td style=&quot;color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #ffe49c; vertical-align: top; white-space: pre-wrap;&quot;&gt;&lt;div&gt;[[File:fse-prestressed-concrete-in-fire-v3.svg|thumb|upright=1.5|alt=Prestressed concrete in fire: testing and fire-resistance assessment, showing the relationships described in the text.|Testing and fire-resistance assessment in the assessment of &lt;del style=&quot;font-weight: bold; text-decoration: none;&quot;&gt;Prestressed &lt;/del&gt;concrete in fire.]]&lt;/div&gt;&lt;/td&gt;&lt;td class=&quot;diff-marker&quot; data-marker=&quot;+&quot;&gt;&lt;/td&gt;&lt;td style=&quot;color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #a3d3ff; vertical-align: top; white-space: pre-wrap;&quot;&gt;&lt;div&gt;[[File:fse-prestressed-concrete-in-fire-v3.svg|thumb|upright=1.5|alt=Prestressed concrete in fire: testing and fire-resistance assessment, showing the relationships described in the text.|Testing and fire-resistance assessment in the assessment of &lt;ins style=&quot;font-weight: bold; text-decoration: none;&quot;&gt;prestressed &lt;/ins&gt;concrete in fire.]]&lt;/div&gt;&lt;/td&gt;&lt;/tr&gt;
&lt;tr&gt;&lt;td class=&quot;diff-marker&quot;&gt;&lt;/td&gt;&lt;td style=&quot;background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;&quot;&gt;&lt;br&gt;&lt;/td&gt;&lt;td class=&quot;diff-marker&quot;&gt;&lt;/td&gt;&lt;td style=&quot;background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;&quot;&gt;&lt;br&gt;&lt;/td&gt;&lt;/tr&gt;
&lt;tr&gt;&lt;td class=&quot;diff-marker&quot;&gt;&lt;/td&gt;&lt;td style=&quot;background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;&quot;&gt;&lt;div&gt;For standard exposure, empirical methods can relate dimensions and other parameters to results from furnace tests. Nonstandard exposure generally requires a more explicit thermal analysis followed by structural evaluation. Fleischmann and Buchanan describe both approaches and their different information requirements. A correlation derived from a standard test does not independently establish performance for an arbitrary natural fire.&amp;lt;ref name=&amp;quot;concreteinfi_FB_4-239&amp;quot; /&amp;gt;&lt;/div&gt;&lt;/td&gt;&lt;td class=&quot;diff-marker&quot;&gt;&lt;/td&gt;&lt;td style=&quot;background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;&quot;&gt;&lt;div&gt;For standard exposure, empirical methods can relate dimensions and other parameters to results from furnace tests. Nonstandard exposure generally requires a more explicit thermal analysis followed by structural evaluation. Fleischmann and Buchanan describe both approaches and their different information requirements. A correlation derived from a standard test does not independently establish performance for an arbitrary natural fire.&amp;lt;ref name=&amp;quot;concreteinfi_FB_4-239&amp;quot; /&amp;gt;&lt;/div&gt;&lt;/td&gt;&lt;/tr&gt;
&lt;tr&gt;&lt;td class=&quot;diff-marker&quot;&gt;&lt;/td&gt;&lt;td style=&quot;background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;&quot;&gt;&lt;br&gt;&lt;/td&gt;&lt;td class=&quot;diff-marker&quot;&gt;&lt;/td&gt;&lt;td style=&quot;background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;&quot;&gt;&lt;br&gt;&lt;/td&gt;&lt;/tr&gt;
&lt;tr&gt;&lt;td class=&quot;diff-marker&quot;&gt;&lt;/td&gt;&lt;td style=&quot;background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;&quot;&gt;&lt;div&gt;New Zealand&amp;#039;s C/VM2, second edition of 2025, defines a fire resistance rating using three durations, and their order is structural adequacy, integrity and insulation. The definition permits standard testing or a specified calculation method verified against standard fire-resistance tests. This is the terminology of that New Zealand document, rather than a universal notation for every jurisdiction.&amp;lt;ref name=&amp;quot;concreteinfi_CVM_64&amp;quot;&amp;gt;Ministry of Business, Innovation and Employment (2025), p. 64.&amp;lt;/ref&amp;gt;&lt;/div&gt;&lt;/td&gt;&lt;td class=&quot;diff-marker&quot;&gt;&lt;/td&gt;&lt;td style=&quot;background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;&quot;&gt;&lt;div&gt;New Zealand&amp;#039;s C/VM2, second edition of 2025, defines a fire resistance rating using three durations, and their order is structural adequacy, integrity and insulation. The definition permits standard testing or a specified calculation method verified against standard fire-resistance tests. This is the terminology of that New Zealand document, rather than a universal notation for every jurisdiction.&amp;lt;ref name=&amp;quot;concreteinfi_CVM_64&amp;quot;&amp;gt;Ministry of Business, Innovation and Employment (2025), p. 64.&amp;lt;/ref&amp;gt;&lt;/div&gt;&lt;/td&gt;&lt;/tr&gt;
&lt;tr&gt;&lt;td class=&quot;diff-marker&quot; data-marker=&quot;−&quot;&gt;&lt;/td&gt;&lt;td style=&quot;color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #ffe49c; vertical-align: top; white-space: pre-wrap;&quot;&gt;&lt;div&gt;&lt;del style=&quot;font-weight: bold; text-decoration: none;&quot;&gt;&lt;/del&gt;&lt;/div&gt;&lt;/td&gt;&lt;td colspan=&quot;2&quot; class=&quot;diff-side-added&quot;&gt;&lt;/td&gt;&lt;/tr&gt;
&lt;tr&gt;&lt;td class=&quot;diff-marker&quot; data-marker=&quot;−&quot;&gt;&lt;/td&gt;&lt;td style=&quot;color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #ffe49c; vertical-align: top; white-space: pre-wrap;&quot;&gt;&lt;div&gt;&lt;del style=&quot;font-weight: bold; text-decoration: none;&quot;&gt;== See also ==&lt;/del&gt;&lt;/div&gt;&lt;/td&gt;&lt;td colspan=&quot;2&quot; class=&quot;diff-side-added&quot;&gt;&lt;/td&gt;&lt;/tr&gt;
&lt;tr&gt;&lt;td class=&quot;diff-marker&quot; data-marker=&quot;−&quot;&gt;&lt;/td&gt;&lt;td style=&quot;color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #ffe49c; vertical-align: top; white-space: pre-wrap;&quot;&gt;&lt;div&gt;&lt;del style=&quot;font-weight: bold; text-decoration: none;&quot;&gt;&lt;/del&gt;&lt;/div&gt;&lt;/td&gt;&lt;td colspan=&quot;2&quot; class=&quot;diff-side-added&quot;&gt;&lt;/td&gt;&lt;/tr&gt;
&lt;tr&gt;&lt;td class=&quot;diff-marker&quot; data-marker=&quot;−&quot;&gt;&lt;/td&gt;&lt;td style=&quot;color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #ffe49c; vertical-align: top; white-space: pre-wrap;&quot;&gt;&lt;div&gt;&lt;del style=&quot;font-weight: bold; text-decoration: none;&quot;&gt;&lt;/del&gt;&lt;/div&gt;&lt;/td&gt;&lt;td colspan=&quot;2&quot; class=&quot;diff-side-added&quot;&gt;&lt;/td&gt;&lt;/tr&gt;
&lt;tr&gt;&lt;td class=&quot;diff-marker&quot;&gt;&lt;/td&gt;&lt;td style=&quot;background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;&quot;&gt;&lt;br&gt;&lt;/td&gt;&lt;td class=&quot;diff-marker&quot;&gt;&lt;/td&gt;&lt;td style=&quot;background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;&quot;&gt;&lt;br&gt;&lt;/td&gt;&lt;/tr&gt;
&lt;tr&gt;&lt;td class=&quot;diff-marker&quot;&gt;&lt;/td&gt;&lt;td style=&quot;background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;&quot;&gt;&lt;div&gt;== Notes ==&lt;/div&gt;&lt;/td&gt;&lt;td class=&quot;diff-marker&quot;&gt;&lt;/td&gt;&lt;td style=&quot;background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;&quot;&gt;&lt;div&gt;== Notes ==&lt;/div&gt;&lt;/td&gt;&lt;/tr&gt;

&lt;!-- diff cache key firesb_pjbsiy42-wiki_:diff:1.41:old-8514:rev-9481:php=table --&gt;
&lt;/table&gt;</summary>
		<author><name>Peter</name></author>
	</entry>
	<entry>
		<id>https://fire-safety.academy/w/index.php?title=Prestressed_concrete_in_fire&amp;diff=8514&amp;oldid=prev</id>
		<title>Thomas: Add SVG figures fse-prestressed-concrete-in-fire-v1.svg, fse-prestressed-concrete-in-fire-v2.svg, fse-prestressed-concrete-in-fire-v3.svg (list-6 visual plan)</title>
		<link rel="alternate" type="text/html" href="https://fire-safety.academy/w/index.php?title=Prestressed_concrete_in_fire&amp;diff=8514&amp;oldid=prev"/>
		<updated>2026-11-13T08:31:28Z</updated>

		<summary type="html">&lt;p&gt;Add SVG figures fse-prestressed-concrete-in-fire-v1.svg, fse-prestressed-concrete-in-fire-v2.svg, fse-prestressed-concrete-in-fire-v3.svg (list-6 visual plan)&lt;/p&gt;
&lt;table style=&quot;background-color: #fff; color: #202122;&quot; data-mw=&quot;interface&quot;&gt;
				&lt;col class=&quot;diff-marker&quot; /&gt;
				&lt;col class=&quot;diff-content&quot; /&gt;
				&lt;col class=&quot;diff-marker&quot; /&gt;
				&lt;col class=&quot;diff-content&quot; /&gt;
				&lt;tr class=&quot;diff-title&quot; lang=&quot;en&quot;&gt;
				&lt;td colspan=&quot;2&quot; style=&quot;background-color: #fff; color: #202122; text-align: center;&quot;&gt;← Older revision&lt;/td&gt;
				&lt;td colspan=&quot;2&quot; style=&quot;background-color: #fff; color: #202122; text-align: center;&quot;&gt;Revision as of 09:31, 13 November 2026&lt;/td&gt;
				&lt;/tr&gt;&lt;tr&gt;&lt;td colspan=&quot;2&quot; class=&quot;diff-lineno&quot; id=&quot;mw-diff-left-l8&quot;&gt;Line 8:&lt;/td&gt;
&lt;td colspan=&quot;2&quot; class=&quot;diff-lineno&quot;&gt;Line 8:&lt;/td&gt;&lt;/tr&gt;
&lt;tr&gt;&lt;td class=&quot;diff-marker&quot;&gt;&lt;/td&gt;&lt;td style=&quot;background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;&quot;&gt;&lt;br&gt;&lt;/td&gt;&lt;td class=&quot;diff-marker&quot;&gt;&lt;/td&gt;&lt;td style=&quot;background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;&quot;&gt;&lt;br&gt;&lt;/td&gt;&lt;/tr&gt;
&lt;tr&gt;&lt;td class=&quot;diff-marker&quot;&gt;&lt;/td&gt;&lt;td style=&quot;background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;&quot;&gt;&lt;div&gt;Prestressing introduces forces before the member carries its full service loading; the NFPA handbook explains that the steel therefore begins fire exposure under substantial initial stress. Heating changes its strength, stiffness and time-dependent deformation. These effects can reduce the prestressing force and the capacity of the complete member.&amp;lt;ref name=&amp;quot;NFPA-§19.2,p.19-53&amp;quot;&amp;gt;Cote et al. (2008), §19.2, p. 19-53.&amp;lt;/ref&amp;gt;&lt;/div&gt;&lt;/td&gt;&lt;td class=&quot;diff-marker&quot;&gt;&lt;/td&gt;&lt;td style=&quot;background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;&quot;&gt;&lt;div&gt;Prestressing introduces forces before the member carries its full service loading; the NFPA handbook explains that the steel therefore begins fire exposure under substantial initial stress. Heating changes its strength, stiffness and time-dependent deformation. These effects can reduce the prestressing force and the capacity of the complete member.&amp;lt;ref name=&amp;quot;NFPA-§19.2,p.19-53&amp;quot;&amp;gt;Cote et al. (2008), §19.2, p. 19-53.&amp;lt;/ref&amp;gt;&lt;/div&gt;&lt;/td&gt;&lt;/tr&gt;
&lt;tr&gt;&lt;td colspan=&quot;2&quot; class=&quot;diff-side-deleted&quot;&gt;&lt;/td&gt;&lt;td class=&quot;diff-marker&quot; data-marker=&quot;+&quot;&gt;&lt;/td&gt;&lt;td style=&quot;color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #a3d3ff; vertical-align: top; white-space: pre-wrap;&quot;&gt;&lt;div&gt;&lt;ins style=&quot;font-weight: bold; text-decoration: none;&quot;&gt;[[File:fse-prestressed-concrete-in-fire-v1.svg|thumb|upright=1.5|alt=Prestressed concrete in fire: prestress, heating and the resisting system, showing the relationships described in the text.|Prestress, heating and the resisting system in the assessment of Prestressed concrete in fire.]]&lt;/ins&gt;&lt;/div&gt;&lt;/td&gt;&lt;/tr&gt;
&lt;tr&gt;&lt;td class=&quot;diff-marker&quot;&gt;&lt;/td&gt;&lt;td style=&quot;background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;&quot;&gt;&lt;br&gt;&lt;/td&gt;&lt;td class=&quot;diff-marker&quot;&gt;&lt;/td&gt;&lt;td style=&quot;background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;&quot;&gt;&lt;br&gt;&lt;/td&gt;&lt;/tr&gt;
&lt;tr&gt;&lt;td class=&quot;diff-marker&quot;&gt;&lt;/td&gt;&lt;td style=&quot;background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;&quot;&gt;&lt;div&gt;The distinction from ordinary reinforced concrete is not simply a different concrete strength. The function and type of steel matter, as do the initial force and its transfer into the concrete. [[Strength reduction at elevated temperatures]] must therefore be represented for the actual tendon material. A relationship for ordinary hot-rolled reinforcement does not establish every prestressing-steel response.&amp;lt;ref name=&amp;quot;NFPA-§19.2,pp.19-53-19-54&amp;quot; /&amp;gt;&lt;/div&gt;&lt;/td&gt;&lt;td class=&quot;diff-marker&quot;&gt;&lt;/td&gt;&lt;td style=&quot;background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;&quot;&gt;&lt;div&gt;The distinction from ordinary reinforced concrete is not simply a different concrete strength. The function and type of steel matter, as do the initial force and its transfer into the concrete. [[Strength reduction at elevated temperatures]] must therefore be represented for the actual tendon material. A relationship for ordinary hot-rolled reinforcement does not establish every prestressing-steel response.&amp;lt;ref name=&amp;quot;NFPA-§19.2,pp.19-53-19-54&amp;quot; /&amp;gt;&lt;/div&gt;&lt;/td&gt;&lt;/tr&gt;
&lt;tr&gt;&lt;td colspan=&quot;2&quot; class=&quot;diff-lineno&quot; id=&quot;mw-diff-left-l18&quot;&gt;Line 18:&lt;/td&gt;
&lt;td colspan=&quot;2&quot; class=&quot;diff-lineno&quot;&gt;Line 19:&lt;/td&gt;&lt;/tr&gt;
&lt;tr&gt;&lt;td class=&quot;diff-marker&quot;&gt;&lt;/td&gt;&lt;td style=&quot;background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;&quot;&gt;&lt;br&gt;&lt;/td&gt;&lt;td class=&quot;diff-marker&quot;&gt;&lt;/td&gt;&lt;td style=&quot;background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;&quot;&gt;&lt;br&gt;&lt;/td&gt;&lt;/tr&gt;
&lt;tr&gt;&lt;td class=&quot;diff-marker&quot;&gt;&lt;/td&gt;&lt;td style=&quot;background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;&quot;&gt;&lt;div&gt;Cover is part of the thermal protection around the steel. Its effectiveness depends on remaining in place and on the distance from the exposed face to the tendon. The NFPA handbook notes that spalling can expose prestressing steel directly. The member then has both a changed cross-section and a changed heating boundary.&amp;lt;ref name=&amp;quot;NFPA-§19.2,pp.19-53-19-54&amp;quot; /&amp;gt;&lt;/div&gt;&lt;/td&gt;&lt;td class=&quot;diff-marker&quot;&gt;&lt;/td&gt;&lt;td style=&quot;background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;&quot;&gt;&lt;div&gt;Cover is part of the thermal protection around the steel. Its effectiveness depends on remaining in place and on the distance from the exposed face to the tendon. The NFPA handbook notes that spalling can expose prestressing steel directly. The member then has both a changed cross-section and a changed heating boundary.&amp;lt;ref name=&amp;quot;NFPA-§19.2,pp.19-53-19-54&amp;quot; /&amp;gt;&lt;/div&gt;&lt;/td&gt;&lt;/tr&gt;
&lt;tr&gt;&lt;td colspan=&quot;2&quot; class=&quot;diff-side-deleted&quot;&gt;&lt;/td&gt;&lt;td class=&quot;diff-marker&quot; data-marker=&quot;+&quot;&gt;&lt;/td&gt;&lt;td style=&quot;color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #a3d3ff; vertical-align: top; white-space: pre-wrap;&quot;&gt;&lt;div&gt;&lt;ins style=&quot;font-weight: bold; text-decoration: none;&quot;&gt;[[File:fse-prestressed-concrete-in-fire-v2.svg|thumb|upright=1.5|alt=Prestressed concrete in fire: cover, connections and the condition after cooling, showing the relationships described in the text.|Cover, connections and the condition after cooling in the assessment of Prestressed concrete in fire.]]&lt;/ins&gt;&lt;/div&gt;&lt;/td&gt;&lt;/tr&gt;
&lt;tr&gt;&lt;td class=&quot;diff-marker&quot;&gt;&lt;/td&gt;&lt;td style=&quot;background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;&quot;&gt;&lt;br&gt;&lt;/td&gt;&lt;td class=&quot;diff-marker&quot;&gt;&lt;/td&gt;&lt;td style=&quot;background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;&quot;&gt;&lt;br&gt;&lt;/td&gt;&lt;/tr&gt;
&lt;tr&gt;&lt;td class=&quot;diff-marker&quot;&gt;&lt;/td&gt;&lt;td style=&quot;background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;&quot;&gt;&lt;div&gt;A floor or roof is also a system of members and supports. Precast elements, bearings and connections have different dependencies from a continuous cast-in-place arrangement. The handbook&amp;#039;s firefighting discussion explains that roof loss can remove restraint from heavy wall panels. The structural consequences can extend beyond the heated concrete element.&amp;lt;ref name=&amp;quot;NFPA-§12.8,p.12-136&amp;quot;&amp;gt;Cote et al. (2008), §12.8, p. 12-136.&amp;lt;/ref&amp;gt;&lt;/div&gt;&lt;/td&gt;&lt;td class=&quot;diff-marker&quot;&gt;&lt;/td&gt;&lt;td style=&quot;background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;&quot;&gt;&lt;div&gt;A floor or roof is also a system of members and supports. Precast elements, bearings and connections have different dependencies from a continuous cast-in-place arrangement. The handbook&amp;#039;s firefighting discussion explains that roof loss can remove restraint from heavy wall panels. The structural consequences can extend beyond the heated concrete element.&amp;lt;ref name=&amp;quot;NFPA-§12.8,p.12-136&amp;quot;&amp;gt;Cote et al. (2008), §12.8, p. 12-136.&amp;lt;/ref&amp;gt;&lt;/div&gt;&lt;/td&gt;&lt;/tr&gt;
&lt;tr&gt;&lt;td colspan=&quot;2&quot; class=&quot;diff-lineno&quot; id=&quot;mw-diff-left-l106&quot;&gt;Line 106:&lt;/td&gt;
&lt;td colspan=&quot;2&quot; class=&quot;diff-lineno&quot;&gt;Line 108:&lt;/td&gt;&lt;/tr&gt;
&lt;tr&gt;&lt;td class=&quot;diff-marker&quot;&gt;&lt;/td&gt;&lt;td style=&quot;background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;&quot;&gt;&lt;br&gt;&lt;/td&gt;&lt;td class=&quot;diff-marker&quot;&gt;&lt;/td&gt;&lt;td style=&quot;background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;&quot;&gt;&lt;br&gt;&lt;/td&gt;&lt;/tr&gt;
&lt;tr&gt;&lt;td class=&quot;diff-marker&quot;&gt;&lt;/td&gt;&lt;td style=&quot;background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;&quot;&gt;&lt;div&gt;Fire resistance is evaluated against specified functions under a defined exposure. A separating concrete floor may need to support loads and limit heat transfer to the space above; a column has a different structural role and exposure arrangement. The required endpoints follow the assembly and assessment method, rather than the material name alone.&amp;lt;ref name=&amp;quot;concreteinfi_FB_4-239&amp;quot; /&amp;gt;&amp;lt;ref name=&amp;quot;concreteinfi_FB_4-242&amp;quot; /&amp;gt;&lt;/div&gt;&lt;/td&gt;&lt;td class=&quot;diff-marker&quot;&gt;&lt;/td&gt;&lt;td style=&quot;background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;&quot;&gt;&lt;div&gt;Fire resistance is evaluated against specified functions under a defined exposure. A separating concrete floor may need to support loads and limit heat transfer to the space above; a column has a different structural role and exposure arrangement. The required endpoints follow the assembly and assessment method, rather than the material name alone.&amp;lt;ref name=&amp;quot;concreteinfi_FB_4-239&amp;quot; /&amp;gt;&amp;lt;ref name=&amp;quot;concreteinfi_FB_4-242&amp;quot; /&amp;gt;&lt;/div&gt;&lt;/td&gt;&lt;/tr&gt;
&lt;tr&gt;&lt;td colspan=&quot;2&quot; class=&quot;diff-side-deleted&quot;&gt;&lt;/td&gt;&lt;td class=&quot;diff-marker&quot; data-marker=&quot;+&quot;&gt;&lt;/td&gt;&lt;td style=&quot;color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #a3d3ff; vertical-align: top; white-space: pre-wrap;&quot;&gt;&lt;div&gt;&lt;ins style=&quot;font-weight: bold; text-decoration: none;&quot;&gt;[[File:fse-prestressed-concrete-in-fire-v3.svg|thumb|upright=1.5|alt=Prestressed concrete in fire: testing and fire-resistance assessment, showing the relationships described in the text.|Testing and fire-resistance assessment in the assessment of Prestressed concrete in fire.]]&lt;/ins&gt;&lt;/div&gt;&lt;/td&gt;&lt;/tr&gt;
&lt;tr&gt;&lt;td class=&quot;diff-marker&quot;&gt;&lt;/td&gt;&lt;td style=&quot;background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;&quot;&gt;&lt;br&gt;&lt;/td&gt;&lt;td class=&quot;diff-marker&quot;&gt;&lt;/td&gt;&lt;td style=&quot;background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;&quot;&gt;&lt;br&gt;&lt;/td&gt;&lt;/tr&gt;
&lt;tr&gt;&lt;td class=&quot;diff-marker&quot;&gt;&lt;/td&gt;&lt;td style=&quot;background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;&quot;&gt;&lt;div&gt;For standard exposure, empirical methods can relate dimensions and other parameters to results from furnace tests. Nonstandard exposure generally requires a more explicit thermal analysis followed by structural evaluation. Fleischmann and Buchanan describe both approaches and their different information requirements. A correlation derived from a standard test does not independently establish performance for an arbitrary natural fire.&amp;lt;ref name=&amp;quot;concreteinfi_FB_4-239&amp;quot; /&amp;gt;&lt;/div&gt;&lt;/td&gt;&lt;td class=&quot;diff-marker&quot;&gt;&lt;/td&gt;&lt;td style=&quot;background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;&quot;&gt;&lt;div&gt;For standard exposure, empirical methods can relate dimensions and other parameters to results from furnace tests. Nonstandard exposure generally requires a more explicit thermal analysis followed by structural evaluation. Fleischmann and Buchanan describe both approaches and their different information requirements. A correlation derived from a standard test does not independently establish performance for an arbitrary natural fire.&amp;lt;ref name=&amp;quot;concreteinfi_FB_4-239&amp;quot; /&amp;gt;&lt;/div&gt;&lt;/td&gt;&lt;/tr&gt;

&lt;!-- diff cache key firesb_pjbsiy42-wiki_:diff:1.41:old-4104:rev-8514:php=table --&gt;
&lt;/table&gt;</summary>
		<author><name>Thomas</name></author>
	</entry>
	<entry>
		<id>https://fire-safety.academy/w/index.php?title=Prestressed_concrete_in_fire&amp;diff=4104&amp;oldid=prev</id>
		<title>Linda: Source and style review: Prestressed concrete in fire (written by GPT-6)</title>
		<link rel="alternate" type="text/html" href="https://fire-safety.academy/w/index.php?title=Prestressed_concrete_in_fire&amp;diff=4104&amp;oldid=prev"/>
		<updated>2026-11-07T22:14:02Z</updated>

		<summary type="html">&lt;p&gt;Source and style review: Prestressed concrete in fire (written by GPT-6)&lt;/p&gt;
&lt;table style=&quot;background-color: #fff; color: #202122;&quot; data-mw=&quot;interface&quot;&gt;
				&lt;col class=&quot;diff-marker&quot; /&gt;
				&lt;col class=&quot;diff-content&quot; /&gt;
				&lt;col class=&quot;diff-marker&quot; /&gt;
				&lt;col class=&quot;diff-content&quot; /&gt;
				&lt;tr class=&quot;diff-title&quot; lang=&quot;en&quot;&gt;
				&lt;td colspan=&quot;2&quot; style=&quot;background-color: #fff; color: #202122; text-align: center;&quot;&gt;← Older revision&lt;/td&gt;
				&lt;td colspan=&quot;2&quot; style=&quot;background-color: #fff; color: #202122; text-align: center;&quot;&gt;Revision as of 23:14, 7 November 2026&lt;/td&gt;
				&lt;/tr&gt;&lt;tr&gt;&lt;td colspan=&quot;2&quot; class=&quot;diff-lineno&quot; id=&quot;mw-diff-left-l1&quot;&gt;Line 1:&lt;/td&gt;
&lt;td colspan=&quot;2&quot; class=&quot;diff-lineno&quot;&gt;Line 1:&lt;/td&gt;&lt;/tr&gt;
&lt;tr&gt;&lt;td class=&quot;diff-marker&quot; data-marker=&quot;−&quot;&gt;&lt;/td&gt;&lt;td style=&quot;color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #ffe49c; vertical-align: top; white-space: pre-wrap;&quot;&gt;&lt;div&gt;&#039;&#039;&#039;Prestressed [[Concrete in fire|concrete in fire]]&#039;&#039;&#039; concerns the response of concrete members containing deliberately tensioned steel when they are heated by a fire. Their resistance depends on the temperatures and properties of both concrete and steel, together with the force initially introduced by prestressing. The SFPE Handbook treats reinforcement temperature and structural continuity as parts of the member assessment.&amp;lt;ref name=&quot;FB-pre&quot;&amp;gt;Fleischmann and Buchanan (2002), pp. 4-239–4-246.&amp;lt;/ref&amp;gt;&amp;lt;ref name=&quot;NFPA-§19.2,pp.19-53-19-54&quot;&amp;gt;Cote et al. (2008), §19.2, pp. 19-53–19-54.&amp;lt;/ref&amp;gt;&lt;/div&gt;&lt;/td&gt;&lt;td class=&quot;diff-marker&quot; data-marker=&quot;+&quot;&gt;&lt;/td&gt;&lt;td style=&quot;color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #a3d3ff; vertical-align: top; white-space: pre-wrap;&quot;&gt;&lt;div&gt;&#039;&#039;&#039;Prestressed [[Concrete in fire|concrete in fire]]&#039;&#039;&#039; concerns the response of concrete members containing deliberately tensioned steel when they are heated by a fire. Their resistance depends on the temperatures and properties of both concrete and steel, together with the force initially introduced by prestressing. The &lt;ins style=&quot;font-weight: bold; text-decoration: none;&quot;&gt;Society of Fire Protection Engineers (&lt;/ins&gt;SFPE&lt;ins style=&quot;font-weight: bold; text-decoration: none;&quot;&gt;) &lt;/ins&gt;Handbook treats reinforcement temperature and structural continuity as parts of the member assessment.&amp;lt;ref name=&quot;FB-pre&quot;&amp;gt;Fleischmann and Buchanan (2002), pp. 4-239–4-246.&amp;lt;/ref&amp;gt;&amp;lt;ref name=&quot;NFPA-§19.2,pp.19-53-19-54&quot;&amp;gt;Cote et al. (2008), §19.2, pp. 19-53–19-54.&amp;lt;/ref&amp;gt;&lt;/div&gt;&lt;/td&gt;&lt;/tr&gt;
&lt;tr&gt;&lt;td class=&quot;diff-marker&quot;&gt;&lt;/td&gt;&lt;td style=&quot;background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;&quot;&gt;&lt;br&gt;&lt;/td&gt;&lt;td class=&quot;diff-marker&quot;&gt;&lt;/td&gt;&lt;td style=&quot;background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;&quot;&gt;&lt;br&gt;&lt;/td&gt;&lt;/tr&gt;
&lt;tr&gt;&lt;td class=&quot;diff-marker&quot; data-marker=&quot;−&quot;&gt;&lt;/td&gt;&lt;td style=&quot;color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #ffe49c; vertical-align: top; white-space: pre-wrap;&quot;&gt;&lt;div&gt;Concrete cover delays heating of embedded steel, but it does not prevent heating indefinitely. [[Spalling]] can remove that protection and change the exposed geometry&lt;del style=&quot;font-weight: bold; text-decoration: none;&quot;&gt;; the &lt;/del&gt;NFPA Fire Protection Handbook gives particular attention to the initial stress and temperature sensitivity of prestressing steel. Those characteristics distinguish its response from an otherwise similar member with ordinary reinforcement.&amp;lt;ref name=&quot;NFPA-§19.2,pp.19-53-19-54&quot; /&amp;gt;&lt;/div&gt;&lt;/td&gt;&lt;td class=&quot;diff-marker&quot; data-marker=&quot;+&quot;&gt;&lt;/td&gt;&lt;td style=&quot;color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #a3d3ff; vertical-align: top; white-space: pre-wrap;&quot;&gt;&lt;div&gt;Concrete cover delays heating of embedded steel, but it does not prevent heating indefinitely. [[Spalling]] can remove that protection and change the exposed geometry&lt;ins style=&quot;font-weight: bold; text-decoration: none;&quot;&gt;. The National Fire Protection Association (&lt;/ins&gt;NFPA&lt;ins style=&quot;font-weight: bold; text-decoration: none;&quot;&gt;) &lt;/ins&gt;Fire Protection Handbook gives particular attention to the initial stress and temperature sensitivity of prestressing steel. Those characteristics distinguish its response from an otherwise similar member with ordinary reinforcement.&amp;lt;ref name=&quot;NFPA-§19.2,pp.19-53-19-54&quot; /&amp;gt;&lt;/div&gt;&lt;/td&gt;&lt;/tr&gt;
&lt;tr&gt;&lt;td class=&quot;diff-marker&quot;&gt;&lt;/td&gt;&lt;td style=&quot;background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;&quot;&gt;&lt;br&gt;&lt;/td&gt;&lt;td class=&quot;diff-marker&quot;&gt;&lt;/td&gt;&lt;td style=&quot;background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;&quot;&gt;&lt;br&gt;&lt;/td&gt;&lt;/tr&gt;
&lt;tr&gt;&lt;td class=&quot;diff-marker&quot;&gt;&lt;/td&gt;&lt;td style=&quot;background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;&quot;&gt;&lt;div&gt;The assessment therefore follows heat transfer, changing material properties and the complete resisting system. A classification as [[Fire-resistive construction|fire-resistive construction]] does not replace these member-specific conditions. Inspection after a fire also has to consider losses that remain after cooling.&amp;lt;ref name=&amp;quot;NFPA-§19.4,pp.19-65,19-73&amp;quot;&amp;gt;Cote et al. (2008), §19.4, pp. 19-65, 19-73.&amp;lt;/ref&amp;gt;&lt;/div&gt;&lt;/td&gt;&lt;td class=&quot;diff-marker&quot;&gt;&lt;/td&gt;&lt;td style=&quot;background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;&quot;&gt;&lt;div&gt;The assessment therefore follows heat transfer, changing material properties and the complete resisting system. A classification as [[Fire-resistive construction|fire-resistive construction]] does not replace these member-specific conditions. Inspection after a fire also has to consider losses that remain after cooling.&amp;lt;ref name=&amp;quot;NFPA-§19.4,pp.19-65,19-73&amp;quot;&amp;gt;Cote et al. (2008), §19.4, pp. 19-65, 19-73.&amp;lt;/ref&amp;gt;&lt;/div&gt;&lt;/td&gt;&lt;/tr&gt;

&lt;!-- diff cache key firesb_pjbsiy42-wiki_:diff:1.41:old-3989:rev-4104:php=table --&gt;
&lt;/table&gt;</summary>
		<author><name>Linda</name></author>
	</entry>
	<entry>
		<id>https://fire-safety.academy/w/index.php?title=Prestressed_concrete_in_fire&amp;diff=3989&amp;oldid=prev</id>
		<title>Linda: Source and style review: Prestressed concrete in fire (written by GPT-6)</title>
		<link rel="alternate" type="text/html" href="https://fire-safety.academy/w/index.php?title=Prestressed_concrete_in_fire&amp;diff=3989&amp;oldid=prev"/>
		<updated>2026-11-07T22:01:56Z</updated>

		<summary type="html">&lt;p&gt;Source and style review: Prestressed concrete in fire (written by GPT-6)&lt;/p&gt;
&lt;table style=&quot;background-color: #fff; color: #202122;&quot; data-mw=&quot;interface&quot;&gt;
				&lt;col class=&quot;diff-marker&quot; /&gt;
				&lt;col class=&quot;diff-content&quot; /&gt;
				&lt;col class=&quot;diff-marker&quot; /&gt;
				&lt;col class=&quot;diff-content&quot; /&gt;
				&lt;tr class=&quot;diff-title&quot; lang=&quot;en&quot;&gt;
				&lt;td colspan=&quot;2&quot; style=&quot;background-color: #fff; color: #202122; text-align: center;&quot;&gt;← Older revision&lt;/td&gt;
				&lt;td colspan=&quot;2&quot; style=&quot;background-color: #fff; color: #202122; text-align: center;&quot;&gt;Revision as of 23:01, 7 November 2026&lt;/td&gt;
				&lt;/tr&gt;&lt;tr&gt;&lt;td colspan=&quot;2&quot; class=&quot;diff-lineno&quot; id=&quot;mw-diff-left-l1&quot;&gt;Line 1:&lt;/td&gt;
&lt;td colspan=&quot;2&quot; class=&quot;diff-lineno&quot;&gt;Line 1:&lt;/td&gt;&lt;/tr&gt;
&lt;tr&gt;&lt;td class=&quot;diff-marker&quot;&gt;&lt;/td&gt;&lt;td style=&quot;background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;&quot;&gt;&lt;div&gt;&amp;#039;&amp;#039;&amp;#039;Prestressed [[Concrete in fire|concrete in fire]]&amp;#039;&amp;#039;&amp;#039; concerns the response of concrete members containing deliberately tensioned steel when they are heated by a fire. Their resistance depends on the temperatures and properties of both concrete and steel, together with the force initially introduced by prestressing. The SFPE Handbook treats reinforcement temperature and structural continuity as parts of the member assessment.&amp;lt;ref name=&amp;quot;FB-pre&amp;quot;&amp;gt;Fleischmann and Buchanan (2002), pp. 4-239–4-246.&amp;lt;/ref&amp;gt;&amp;lt;ref name=&amp;quot;NFPA-§19.2,pp.19-53-19-54&amp;quot;&amp;gt;Cote et al. (2008), §19.2, pp. 19-53–19-54.&amp;lt;/ref&amp;gt;&lt;/div&gt;&lt;/td&gt;&lt;td class=&quot;diff-marker&quot;&gt;&lt;/td&gt;&lt;td style=&quot;background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;&quot;&gt;&lt;div&gt;&amp;#039;&amp;#039;&amp;#039;Prestressed [[Concrete in fire|concrete in fire]]&amp;#039;&amp;#039;&amp;#039; concerns the response of concrete members containing deliberately tensioned steel when they are heated by a fire. Their resistance depends on the temperatures and properties of both concrete and steel, together with the force initially introduced by prestressing. The SFPE Handbook treats reinforcement temperature and structural continuity as parts of the member assessment.&amp;lt;ref name=&amp;quot;FB-pre&amp;quot;&amp;gt;Fleischmann and Buchanan (2002), pp. 4-239–4-246.&amp;lt;/ref&amp;gt;&amp;lt;ref name=&amp;quot;NFPA-§19.2,pp.19-53-19-54&amp;quot;&amp;gt;Cote et al. (2008), §19.2, pp. 19-53–19-54.&amp;lt;/ref&amp;gt;&lt;/div&gt;&lt;/td&gt;&lt;/tr&gt;
&lt;tr&gt;&lt;td class=&quot;diff-marker&quot;&gt;&lt;/td&gt;&lt;td style=&quot;background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;&quot;&gt;&lt;br&gt;&lt;/td&gt;&lt;td class=&quot;diff-marker&quot;&gt;&lt;/td&gt;&lt;td style=&quot;background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;&quot;&gt;&lt;br&gt;&lt;/td&gt;&lt;/tr&gt;
&lt;tr&gt;&lt;td class=&quot;diff-marker&quot; data-marker=&quot;−&quot;&gt;&lt;/td&gt;&lt;td style=&quot;color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #ffe49c; vertical-align: top; white-space: pre-wrap;&quot;&gt;&lt;div&gt;Concrete cover delays heating of embedded steel, but it does not prevent heating indefinitely. [[Spalling]] can remove that protection and change the exposed geometry&lt;del style=&quot;font-weight: bold; text-decoration: none;&quot;&gt;. The &lt;/del&gt;NFPA Fire Protection Handbook gives particular attention to the initial stress and temperature sensitivity of prestressing steel. Those characteristics distinguish its response from an otherwise similar member with ordinary reinforcement.&amp;lt;ref name=&quot;NFPA-§19.2,pp.19-53-19-54&quot; /&amp;gt;&lt;/div&gt;&lt;/td&gt;&lt;td class=&quot;diff-marker&quot; data-marker=&quot;+&quot;&gt;&lt;/td&gt;&lt;td style=&quot;color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #a3d3ff; vertical-align: top; white-space: pre-wrap;&quot;&gt;&lt;div&gt;Concrete cover delays heating of embedded steel, but it does not prevent heating indefinitely. [[Spalling]] can remove that protection and change the exposed geometry&lt;ins style=&quot;font-weight: bold; text-decoration: none;&quot;&gt;; the &lt;/ins&gt;NFPA Fire Protection Handbook gives particular attention to the initial stress and temperature sensitivity of prestressing steel. Those characteristics distinguish its response from an otherwise similar member with ordinary reinforcement.&amp;lt;ref name=&quot;NFPA-§19.2,pp.19-53-19-54&quot; /&amp;gt;&lt;/div&gt;&lt;/td&gt;&lt;/tr&gt;
&lt;tr&gt;&lt;td class=&quot;diff-marker&quot;&gt;&lt;/td&gt;&lt;td style=&quot;background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;&quot;&gt;&lt;br&gt;&lt;/td&gt;&lt;td class=&quot;diff-marker&quot;&gt;&lt;/td&gt;&lt;td style=&quot;background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;&quot;&gt;&lt;br&gt;&lt;/td&gt;&lt;/tr&gt;
&lt;tr&gt;&lt;td class=&quot;diff-marker&quot;&gt;&lt;/td&gt;&lt;td style=&quot;background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;&quot;&gt;&lt;div&gt;The assessment therefore follows heat transfer, changing material properties and the complete resisting system. A classification as [[Fire-resistive construction|fire-resistive construction]] does not replace these member-specific conditions. Inspection after a fire also has to consider losses that remain after cooling.&amp;lt;ref name=&amp;quot;NFPA-§19.4,pp.19-65,19-73&amp;quot;&amp;gt;Cote et al. (2008), §19.4, pp. 19-65, 19-73.&amp;lt;/ref&amp;gt;&lt;/div&gt;&lt;/td&gt;&lt;td class=&quot;diff-marker&quot;&gt;&lt;/td&gt;&lt;td style=&quot;background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;&quot;&gt;&lt;div&gt;The assessment therefore follows heat transfer, changing material properties and the complete resisting system. A classification as [[Fire-resistive construction|fire-resistive construction]] does not replace these member-specific conditions. Inspection after a fire also has to consider losses that remain after cooling.&amp;lt;ref name=&amp;quot;NFPA-§19.4,pp.19-65,19-73&amp;quot;&amp;gt;Cote et al. (2008), §19.4, pp. 19-65, 19-73.&amp;lt;/ref&amp;gt;&lt;/div&gt;&lt;/td&gt;&lt;/tr&gt;
&lt;tr&gt;&lt;td colspan=&quot;2&quot; class=&quot;diff-lineno&quot; id=&quot;mw-diff-left-l7&quot;&gt;Line 7:&lt;/td&gt;
&lt;td colspan=&quot;2&quot; class=&quot;diff-lineno&quot;&gt;Line 7:&lt;/td&gt;&lt;/tr&gt;
&lt;tr&gt;&lt;td class=&quot;diff-marker&quot;&gt;&lt;/td&gt;&lt;td style=&quot;background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;&quot;&gt;&lt;div&gt;== Prestress, heating and the resisting system ==&lt;/div&gt;&lt;/td&gt;&lt;td class=&quot;diff-marker&quot;&gt;&lt;/td&gt;&lt;td style=&quot;background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;&quot;&gt;&lt;div&gt;== Prestress, heating and the resisting system ==&lt;/div&gt;&lt;/td&gt;&lt;/tr&gt;
&lt;tr&gt;&lt;td class=&quot;diff-marker&quot;&gt;&lt;/td&gt;&lt;td style=&quot;background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;&quot;&gt;&lt;br&gt;&lt;/td&gt;&lt;td class=&quot;diff-marker&quot;&gt;&lt;/td&gt;&lt;td style=&quot;background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;&quot;&gt;&lt;br&gt;&lt;/td&gt;&lt;/tr&gt;
&lt;tr&gt;&lt;td class=&quot;diff-marker&quot; data-marker=&quot;−&quot;&gt;&lt;/td&gt;&lt;td style=&quot;color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #ffe49c; vertical-align: top; white-space: pre-wrap;&quot;&gt;&lt;div&gt;Prestressing introduces forces before the member carries its full service loading&lt;del style=&quot;font-weight: bold; text-decoration: none;&quot;&gt;. The &lt;/del&gt;NFPA handbook explains that the steel therefore begins fire exposure under substantial initial stress. Heating changes its strength, stiffness and time-dependent deformation. These effects can reduce the prestressing force and the capacity of the complete member.&amp;lt;ref name=&quot;NFPA-§19.2,p.19-53&quot;&amp;gt;Cote et al. (2008), §19.2, p. 19-53.&amp;lt;/ref&amp;gt;&lt;/div&gt;&lt;/td&gt;&lt;td class=&quot;diff-marker&quot; data-marker=&quot;+&quot;&gt;&lt;/td&gt;&lt;td style=&quot;color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #a3d3ff; vertical-align: top; white-space: pre-wrap;&quot;&gt;&lt;div&gt;Prestressing introduces forces before the member carries its full service loading&lt;ins style=&quot;font-weight: bold; text-decoration: none;&quot;&gt;; the &lt;/ins&gt;NFPA handbook explains that the steel therefore begins fire exposure under substantial initial stress. Heating changes its strength, stiffness and time-dependent deformation. These effects can reduce the prestressing force and the capacity of the complete member.&amp;lt;ref name=&quot;NFPA-§19.2,p.19-53&quot;&amp;gt;Cote et al. (2008), §19.2, p. 19-53.&amp;lt;/ref&amp;gt;&lt;/div&gt;&lt;/td&gt;&lt;/tr&gt;
&lt;tr&gt;&lt;td class=&quot;diff-marker&quot;&gt;&lt;/td&gt;&lt;td style=&quot;background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;&quot;&gt;&lt;br&gt;&lt;/td&gt;&lt;td class=&quot;diff-marker&quot;&gt;&lt;/td&gt;&lt;td style=&quot;background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;&quot;&gt;&lt;br&gt;&lt;/td&gt;&lt;/tr&gt;
&lt;tr&gt;&lt;td class=&quot;diff-marker&quot;&gt;&lt;/td&gt;&lt;td style=&quot;background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;&quot;&gt;&lt;div&gt;The distinction from ordinary reinforced concrete is not simply a different concrete strength. The function and type of steel matter, as do the initial force and its transfer into the concrete. [[Strength reduction at elevated temperatures]] must therefore be represented for the actual tendon material. A relationship for ordinary hot-rolled reinforcement does not establish every prestressing-steel response.&amp;lt;ref name=&amp;quot;NFPA-§19.2,pp.19-53-19-54&amp;quot; /&amp;gt;&lt;/div&gt;&lt;/td&gt;&lt;td class=&quot;diff-marker&quot;&gt;&lt;/td&gt;&lt;td style=&quot;background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;&quot;&gt;&lt;div&gt;The distinction from ordinary reinforced concrete is not simply a different concrete strength. The function and type of steel matter, as do the initial force and its transfer into the concrete. [[Strength reduction at elevated temperatures]] must therefore be represented for the actual tendon material. A relationship for ordinary hot-rolled reinforcement does not establish every prestressing-steel response.&amp;lt;ref name=&amp;quot;NFPA-§19.2,pp.19-53-19-54&amp;quot; /&amp;gt;&lt;/div&gt;&lt;/td&gt;&lt;/tr&gt;
&lt;tr&gt;&lt;td class=&quot;diff-marker&quot;&gt;&lt;/td&gt;&lt;td style=&quot;background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;&quot;&gt;&lt;br&gt;&lt;/td&gt;&lt;td class=&quot;diff-marker&quot;&gt;&lt;/td&gt;&lt;td style=&quot;background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;&quot;&gt;&lt;br&gt;&lt;/td&gt;&lt;/tr&gt;
&lt;tr&gt;&lt;td class=&quot;diff-marker&quot; data-marker=&quot;−&quot;&gt;&lt;/td&gt;&lt;td style=&quot;color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #ffe49c; vertical-align: top; white-space: pre-wrap;&quot;&gt;&lt;div&gt;Concrete in fire develops temperature gradients because heat enters through exposed surfaces. A tendon close to a heated face can become hotter than reinforcement farther inside. Loss of cover changes that relationship&lt;del style=&quot;font-weight: bold; text-decoration: none;&quot;&gt;. The &lt;/del&gt;SFPE analysis relates reinforcement temperature to the temperature distribution at its depth, while retaining the exposure geometry and member dimensions.&amp;lt;ref name=&quot;FB-pre&quot; /&amp;gt;&lt;/div&gt;&lt;/td&gt;&lt;td class=&quot;diff-marker&quot; data-marker=&quot;+&quot;&gt;&lt;/td&gt;&lt;td style=&quot;color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #a3d3ff; vertical-align: top; white-space: pre-wrap;&quot;&gt;&lt;div&gt;Concrete in fire develops temperature gradients because heat enters through exposed surfaces. A tendon close to a heated face can become hotter than reinforcement farther inside. Loss of cover changes that relationship&lt;ins style=&quot;font-weight: bold; text-decoration: none;&quot;&gt;; the &lt;/ins&gt;SFPE analysis relates reinforcement temperature to the temperature distribution at its depth, while retaining the exposure geometry and member dimensions.&amp;lt;ref name=&quot;FB-pre&quot; /&amp;gt;&lt;/div&gt;&lt;/td&gt;&lt;/tr&gt;
&lt;tr&gt;&lt;td class=&quot;diff-marker&quot;&gt;&lt;/td&gt;&lt;td style=&quot;background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;&quot;&gt;&lt;br&gt;&lt;/td&gt;&lt;td class=&quot;diff-marker&quot;&gt;&lt;/td&gt;&lt;td style=&quot;background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;&quot;&gt;&lt;br&gt;&lt;/td&gt;&lt;/tr&gt;
&lt;tr&gt;&lt;td class=&quot;diff-marker&quot;&gt;&lt;/td&gt;&lt;td style=&quot;background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;&quot;&gt;&lt;div&gt;The [[Load combination for fire|load combination for fire]] defines the external actions to be resisted. Prestress, thermal expansion and restraint then affect how these actions are carried. The NFPA handbook describes upward movement caused by differential thermal expansion as one possible prestressed-member response. The direction of visible movement alone therefore does not establish an uncomplicated bending mechanism.&amp;lt;ref name=&amp;quot;NFPA-§19.2,pp.19-53-19-54&amp;quot; /&amp;gt;&amp;lt;ref name=&amp;quot;NFPA-§19.5,pp.19-93-19-94&amp;quot;&amp;gt;Cote et al. (2008), §19.5, pp. 19-93–19-94.&amp;lt;/ref&amp;gt;&lt;/div&gt;&lt;/td&gt;&lt;td class=&quot;diff-marker&quot;&gt;&lt;/td&gt;&lt;td style=&quot;background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;&quot;&gt;&lt;div&gt;The [[Load combination for fire|load combination for fire]] defines the external actions to be resisted. Prestress, thermal expansion and restraint then affect how these actions are carried. The NFPA handbook describes upward movement caused by differential thermal expansion as one possible prestressed-member response. The direction of visible movement alone therefore does not establish an uncomplicated bending mechanism.&amp;lt;ref name=&amp;quot;NFPA-§19.2,pp.19-53-19-54&amp;quot; /&amp;gt;&amp;lt;ref name=&amp;quot;NFPA-§19.5,pp.19-93-19-94&amp;quot;&amp;gt;Cote et al. (2008), §19.5, pp. 19-93–19-94.&amp;lt;/ref&amp;gt;&lt;/div&gt;&lt;/td&gt;&lt;/tr&gt;
&lt;tr&gt;&lt;td colspan=&quot;2&quot; class=&quot;diff-lineno&quot; id=&quot;mw-diff-left-l67&quot;&gt;Line 67:&lt;/td&gt;
&lt;td colspan=&quot;2&quot; class=&quot;diff-lineno&quot;&gt;Line 67:&lt;/td&gt;&lt;/tr&gt;
&lt;tr&gt;&lt;td class=&quot;diff-marker&quot;&gt;&lt;/td&gt;&lt;td style=&quot;background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;&quot;&gt;&lt;div&gt;== Spalling and loss of cover ==&lt;/div&gt;&lt;/td&gt;&lt;td class=&quot;diff-marker&quot;&gt;&lt;/td&gt;&lt;td style=&quot;background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;&quot;&gt;&lt;div&gt;== Spalling and loss of cover ==&lt;/div&gt;&lt;/td&gt;&lt;/tr&gt;
&lt;tr&gt;&lt;td class=&quot;diff-marker&quot;&gt;&lt;/td&gt;&lt;td style=&quot;background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;&quot;&gt;&lt;br&gt;&lt;/td&gt;&lt;td class=&quot;diff-marker&quot;&gt;&lt;/td&gt;&lt;td style=&quot;background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;&quot;&gt;&lt;br&gt;&lt;/td&gt;&lt;/tr&gt;
&lt;tr&gt;&lt;td class=&quot;diff-marker&quot; data-marker=&quot;−&quot;&gt;&lt;/td&gt;&lt;td style=&quot;color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #ffe49c; vertical-align: top; white-space: pre-wrap;&quot;&gt;&lt;div&gt;Spalling is the breaking away of concrete from the heated surface. Kodur and Harmathy distinguish early explosive loss from later loss associated with weakened material&lt;del style=&quot;font-weight: bold; text-decoration: none;&quot;&gt;. The &lt;/del&gt;process matters because the section can lose both material and thermal protection. Reinforcement formerly enclosed by concrete may then receive more direct heating.&amp;lt;ref name=&quot;concreteinfi_KH_1-163_1-164&quot;&amp;gt;Kodur and Harmathy (2002), pp. 1-163–1-164.&amp;lt;/ref&amp;gt;&lt;/div&gt;&lt;/td&gt;&lt;td class=&quot;diff-marker&quot; data-marker=&quot;+&quot;&gt;&lt;/td&gt;&lt;td style=&quot;color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #a3d3ff; vertical-align: top; white-space: pre-wrap;&quot;&gt;&lt;div&gt;Spalling is the breaking away of concrete from the heated surface. Kodur and Harmathy distinguish early explosive loss from later loss associated with weakened material&lt;ins style=&quot;font-weight: bold; text-decoration: none;&quot;&gt;; the &lt;/ins&gt;process matters because the section can lose both material and thermal protection. Reinforcement formerly enclosed by concrete may then receive more direct heating.&amp;lt;ref name=&quot;concreteinfi_KH_1-163_1-164&quot;&amp;gt;Kodur and Harmathy (2002), pp. 1-163–1-164.&amp;lt;/ref&amp;gt;&lt;/div&gt;&lt;/td&gt;&lt;/tr&gt;
&lt;tr&gt;&lt;td class=&quot;diff-marker&quot;&gt;&lt;/td&gt;&lt;td style=&quot;background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;&quot;&gt;&lt;br&gt;&lt;/td&gt;&lt;td class=&quot;diff-marker&quot;&gt;&lt;/td&gt;&lt;td style=&quot;background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;&quot;&gt;&lt;br&gt;&lt;/td&gt;&lt;/tr&gt;
&lt;tr&gt;&lt;td class=&quot;diff-marker&quot;&gt;&lt;/td&gt;&lt;td style=&quot;background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;&quot;&gt;&lt;div&gt;One proposed mechanism involves moisture movement and pressure within the pores. Heating drives moisture towards cooler regions, where a relatively saturated zone can impede further transport. Pressure can rise if vapour cannot escape readily. The handbook also discusses explanations based on thermal stresses and fracture, so pore pressure is not the sole mechanism considered.&amp;lt;ref name=&amp;quot;concreteinfi_KH_1-163&amp;quot;&amp;gt;Kodur and Harmathy (2002), p. 1-163.&amp;lt;/ref&amp;gt;&lt;/div&gt;&lt;/td&gt;&lt;td class=&quot;diff-marker&quot;&gt;&lt;/td&gt;&lt;td style=&quot;background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;&quot;&gt;&lt;div&gt;One proposed mechanism involves moisture movement and pressure within the pores. Heating drives moisture towards cooler regions, where a relatively saturated zone can impede further transport. Pressure can rise if vapour cannot escape readily. The handbook also discusses explanations based on thermal stresses and fracture, so pore pressure is not the sole mechanism considered.&amp;lt;ref name=&amp;quot;concreteinfi_KH_1-163&amp;quot;&amp;gt;Kodur and Harmathy (2002), p. 1-163.&amp;lt;/ref&amp;gt;&lt;/div&gt;&lt;/td&gt;&lt;/tr&gt;
&lt;tr&gt;&lt;td colspan=&quot;2&quot; class=&quot;diff-lineno&quot; id=&quot;mw-diff-left-l73&quot;&gt;Line 73:&lt;/td&gt;
&lt;td colspan=&quot;2&quot; class=&quot;diff-lineno&quot;&gt;Line 73:&lt;/td&gt;&lt;/tr&gt;
&lt;tr&gt;&lt;td class=&quot;diff-marker&quot;&gt;&lt;/td&gt;&lt;td style=&quot;background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;&quot;&gt;&lt;div&gt;The source illustrates the pressure mechanism using approximately 8 MPa vapour pressure at 300 °C and approximately 5 MPa tensile strength for high-strength concrete. This comparison demonstrates how internal pressure can exceed a resisting tensile stress; it is an explanatory example, not a universal pressure-temperature failure rule. Actual spalling also depends on permeability, moisture, loading and the heating conditions.&amp;lt;ref name=&amp;quot;concreteinfi_KH_1-163_1-164&amp;quot; /&amp;gt;&lt;/div&gt;&lt;/td&gt;&lt;td class=&quot;diff-marker&quot;&gt;&lt;/td&gt;&lt;td style=&quot;background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;&quot;&gt;&lt;div&gt;The source illustrates the pressure mechanism using approximately 8 MPa vapour pressure at 300 °C and approximately 5 MPa tensile strength for high-strength concrete. This comparison demonstrates how internal pressure can exceed a resisting tensile stress; it is an explanatory example, not a universal pressure-temperature failure rule. Actual spalling also depends on permeability, moisture, loading and the heating conditions.&amp;lt;ref name=&amp;quot;concreteinfi_KH_1-163_1-164&amp;quot; /&amp;gt;&lt;/div&gt;&lt;/td&gt;&lt;/tr&gt;
&lt;tr&gt;&lt;td class=&quot;diff-marker&quot;&gt;&lt;/td&gt;&lt;td style=&quot;background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;&quot;&gt;&lt;br&gt;&lt;/td&gt;&lt;td class=&quot;diff-marker&quot;&gt;&lt;/td&gt;&lt;td style=&quot;background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;&quot;&gt;&lt;br&gt;&lt;/td&gt;&lt;/tr&gt;
&lt;tr&gt;&lt;td class=&quot;diff-marker&quot; data-marker=&quot;−&quot;&gt;&lt;/td&gt;&lt;td style=&quot;color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #ffe49c; vertical-align: top; white-space: pre-wrap;&quot;&gt;&lt;div&gt;High compressive strength at room temperature does not by itself prevent spalling. Dense, low-permeability concrete can restrict moisture escape during rapid heating. Once surface material is lost, deeper concrete and reinforcement heat more rapidly&lt;del style=&quot;font-weight: bold; text-decoration: none;&quot;&gt;. A &lt;/del&gt;model that retains the original section throughout the exposure cannot automatically represent that change.&amp;lt;ref name=&quot;concreteinfi_KH_1-163_1-164&quot; /&amp;gt;&lt;/div&gt;&lt;/td&gt;&lt;td class=&quot;diff-marker&quot; data-marker=&quot;+&quot;&gt;&lt;/td&gt;&lt;td style=&quot;color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #a3d3ff; vertical-align: top; white-space: pre-wrap;&quot;&gt;&lt;div&gt;High compressive strength at room temperature does not by itself prevent spalling. Dense, low-permeability concrete can restrict moisture escape during rapid heating. Once surface material is lost, deeper concrete and reinforcement heat more rapidly&lt;ins style=&quot;font-weight: bold; text-decoration: none;&quot;&gt;; a &lt;/ins&gt;model that retains the original section throughout the exposure cannot automatically represent that change.&amp;lt;ref name=&quot;concreteinfi_KH_1-163_1-164&quot; /&amp;gt;&lt;/div&gt;&lt;/td&gt;&lt;/tr&gt;
&lt;tr&gt;&lt;td class=&quot;diff-marker&quot;&gt;&lt;/td&gt;&lt;td style=&quot;background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;&quot;&gt;&lt;br&gt;&lt;/td&gt;&lt;td class=&quot;diff-marker&quot;&gt;&lt;/td&gt;&lt;td style=&quot;background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;&quot;&gt;&lt;br&gt;&lt;/td&gt;&lt;/tr&gt;
&lt;tr&gt;&lt;td class=&quot;diff-marker&quot;&gt;&lt;/td&gt;&lt;td style=&quot;background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;&quot;&gt;&lt;div&gt;Thermal stress offers a different way for cracking to develop. The heated surface tends to expand while cooler material restricts that movement. Kodur and Harmathy discuss fracture-based explanations in which these stresses contribute to surface loss. An analysis based only on vapour pressure therefore addresses one proposed contribution, rather than demonstrating that other mechanisms are absent.&amp;lt;ref name=&amp;quot;concreteinfi_KH_1-163&amp;quot; /&amp;gt;&lt;/div&gt;&lt;/td&gt;&lt;td class=&quot;diff-marker&quot;&gt;&lt;/td&gt;&lt;td style=&quot;background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;&quot;&gt;&lt;div&gt;Thermal stress offers a different way for cracking to develop. The heated surface tends to expand while cooler material restricts that movement. Kodur and Harmathy discuss fracture-based explanations in which these stresses contribute to surface loss. An analysis based only on vapour pressure therefore addresses one proposed contribution, rather than demonstrating that other mechanisms are absent.&amp;lt;ref name=&amp;quot;concreteinfi_KH_1-163&amp;quot; /&amp;gt;&lt;/div&gt;&lt;/td&gt;&lt;/tr&gt;
&lt;tr&gt;&lt;td colspan=&quot;2&quot; class=&quot;diff-lineno&quot; id=&quot;mw-diff-left-l87&quot;&gt;Line 87:&lt;/td&gt;
&lt;td colspan=&quot;2&quot; class=&quot;diff-lineno&quot;&gt;Line 87:&lt;/td&gt;&lt;/tr&gt;
&lt;tr&gt;&lt;td class=&quot;diff-marker&quot;&gt;&lt;/td&gt;&lt;td style=&quot;background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;&quot;&gt;&lt;div&gt;The modulus of elasticity describes stiffness, or resistance to elastic deformation, and it can decrease substantially during heating even when part of the compressive strength remains. Consequently, a strength calculation and a deformation calculation address different effects. Thermal expansion adds another source of deformation and can alter the forces arising in restrained construction.&amp;lt;ref name=&amp;quot;concreteinfi_FB_4-240_4-241&amp;quot; /&amp;gt;&lt;/div&gt;&lt;/td&gt;&lt;td class=&quot;diff-marker&quot;&gt;&lt;/td&gt;&lt;td style=&quot;background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;&quot;&gt;&lt;div&gt;The modulus of elasticity describes stiffness, or resistance to elastic deformation, and it can decrease substantially during heating even when part of the compressive strength remains. Consequently, a strength calculation and a deformation calculation address different effects. Thermal expansion adds another source of deformation and can alter the forces arising in restrained construction.&amp;lt;ref name=&amp;quot;concreteinfi_FB_4-240_4-241&amp;quot; /&amp;gt;&lt;/div&gt;&lt;/td&gt;&lt;/tr&gt;
&lt;tr&gt;&lt;td class=&quot;diff-marker&quot;&gt;&lt;/td&gt;&lt;td style=&quot;background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;&quot;&gt;&lt;br&gt;&lt;/td&gt;&lt;td class=&quot;diff-marker&quot;&gt;&lt;/td&gt;&lt;td style=&quot;background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;&quot;&gt;&lt;br&gt;&lt;/td&gt;&lt;/tr&gt;
&lt;tr&gt;&lt;td class=&quot;diff-marker&quot; data-marker=&quot;−&quot;&gt;&lt;/td&gt;&lt;td style=&quot;color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #ffe49c; vertical-align: top; white-space: pre-wrap;&quot;&gt;&lt;div&gt;In a simplified thermal analysis, the reinforcement temperature may be approximated by the concrete temperature at the bar centre. This connects the heat-transfer calculation to the subsequent structural calculation&lt;del style=&quot;font-weight: bold; text-decoration: none;&quot;&gt;. The &lt;/del&gt;cover depth, exposed faces and heating duration then affect the steel properties used in that analysis. The approximation belongs to the stated modelling approach, rather than every possible member configuration.&amp;lt;ref name=&quot;concreteinfi_FB_4-242&quot; /&amp;gt;&lt;/div&gt;&lt;/td&gt;&lt;td class=&quot;diff-marker&quot; data-marker=&quot;+&quot;&gt;&lt;/td&gt;&lt;td style=&quot;color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #a3d3ff; vertical-align: top; white-space: pre-wrap;&quot;&gt;&lt;div&gt;In a simplified thermal analysis, the reinforcement temperature may be approximated by the concrete temperature at the bar centre. This connects the heat-transfer calculation to the subsequent structural calculation&lt;ins style=&quot;font-weight: bold; text-decoration: none;&quot;&gt;; the &lt;/ins&gt;cover depth, exposed faces and heating duration then affect the steel properties used in that analysis. The approximation belongs to the stated modelling approach, rather than every possible member configuration.&amp;lt;ref name=&quot;concreteinfi_FB_4-242&quot; /&amp;gt;&lt;/div&gt;&lt;/td&gt;&lt;/tr&gt;
&lt;tr&gt;&lt;td class=&quot;diff-marker&quot;&gt;&lt;/td&gt;&lt;td style=&quot;background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;&quot;&gt;&lt;br&gt;&lt;/td&gt;&lt;td class=&quot;diff-marker&quot;&gt;&lt;/td&gt;&lt;td style=&quot;background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;&quot;&gt;&lt;br&gt;&lt;/td&gt;&lt;/tr&gt;
&lt;tr&gt;&lt;td class=&quot;diff-marker&quot;&gt;&lt;/td&gt;&lt;td style=&quot;background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;&quot;&gt;&lt;div&gt;The load present during heating affects how a property curve is established. In the concrete results discussed by Fleischmann and Buchanan, some specimens carried 40% of their compressive strength while being heated. They were then loaded to failure at the temperature of interest. That procedure describes strength while hot, rather than a measurement of residual strength after cooling.&amp;lt;ref name=&amp;quot;concreteinfi_FB_4-240&amp;quot;&amp;gt;Fleischmann and Buchanan (2002), p. 4-240.&amp;lt;/ref&amp;gt;&lt;/div&gt;&lt;/td&gt;&lt;td class=&quot;diff-marker&quot;&gt;&lt;/td&gt;&lt;td style=&quot;background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;&quot;&gt;&lt;div&gt;The load present during heating affects how a property curve is established. In the concrete results discussed by Fleischmann and Buchanan, some specimens carried 40% of their compressive strength while being heated. They were then loaded to failure at the temperature of interest. That procedure describes strength while hot, rather than a measurement of residual strength after cooling.&amp;lt;ref name=&amp;quot;concreteinfi_FB_4-240&amp;quot;&amp;gt;Fleischmann and Buchanan (2002), p. 4-240.&amp;lt;/ref&amp;gt;&lt;/div&gt;&lt;/td&gt;&lt;/tr&gt;
&lt;tr&gt;&lt;td colspan=&quot;2&quot; class=&quot;diff-lineno&quot; id=&quot;mw-diff-left-l105&quot;&gt;Line 105:&lt;/td&gt;
&lt;td colspan=&quot;2&quot; class=&quot;diff-lineno&quot;&gt;Line 105:&lt;/td&gt;&lt;/tr&gt;
&lt;tr&gt;&lt;td class=&quot;diff-marker&quot;&gt;&lt;/td&gt;&lt;td style=&quot;background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;&quot;&gt;&lt;div&gt;== Testing and fire-resistance assessment ==&lt;/div&gt;&lt;/td&gt;&lt;td class=&quot;diff-marker&quot;&gt;&lt;/td&gt;&lt;td style=&quot;background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;&quot;&gt;&lt;div&gt;== Testing and fire-resistance assessment ==&lt;/div&gt;&lt;/td&gt;&lt;/tr&gt;
&lt;tr&gt;&lt;td class=&quot;diff-marker&quot;&gt;&lt;/td&gt;&lt;td style=&quot;background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;&quot;&gt;&lt;br&gt;&lt;/td&gt;&lt;td class=&quot;diff-marker&quot;&gt;&lt;/td&gt;&lt;td style=&quot;background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;&quot;&gt;&lt;br&gt;&lt;/td&gt;&lt;/tr&gt;
&lt;tr&gt;&lt;td class=&quot;diff-marker&quot; data-marker=&quot;−&quot;&gt;&lt;/td&gt;&lt;td style=&quot;color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #ffe49c; vertical-align: top; white-space: pre-wrap;&quot;&gt;&lt;div&gt;Fire resistance is evaluated against specified functions under a defined exposure. A separating concrete floor may need to support loads and limit heat transfer to the space above&lt;del style=&quot;font-weight: bold; text-decoration: none;&quot;&gt;. A &lt;/del&gt;column has a different structural role and exposure arrangement. The required endpoints follow the assembly and assessment method, rather than the material name alone.&amp;lt;ref name=&quot;concreteinfi_FB_4-239&quot; /&amp;gt;&amp;lt;ref name=&quot;concreteinfi_FB_4-242&quot; /&amp;gt;&lt;/div&gt;&lt;/td&gt;&lt;td class=&quot;diff-marker&quot; data-marker=&quot;+&quot;&gt;&lt;/td&gt;&lt;td style=&quot;color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #a3d3ff; vertical-align: top; white-space: pre-wrap;&quot;&gt;&lt;div&gt;Fire resistance is evaluated against specified functions under a defined exposure. A separating concrete floor may need to support loads and limit heat transfer to the space above&lt;ins style=&quot;font-weight: bold; text-decoration: none;&quot;&gt;; a &lt;/ins&gt;column has a different structural role and exposure arrangement. The required endpoints follow the assembly and assessment method, rather than the material name alone.&amp;lt;ref name=&quot;concreteinfi_FB_4-239&quot; /&amp;gt;&amp;lt;ref name=&quot;concreteinfi_FB_4-242&quot; /&amp;gt;&lt;/div&gt;&lt;/td&gt;&lt;/tr&gt;
&lt;tr&gt;&lt;td class=&quot;diff-marker&quot;&gt;&lt;/td&gt;&lt;td style=&quot;background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;&quot;&gt;&lt;br&gt;&lt;/td&gt;&lt;td class=&quot;diff-marker&quot;&gt;&lt;/td&gt;&lt;td style=&quot;background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;&quot;&gt;&lt;br&gt;&lt;/td&gt;&lt;/tr&gt;
&lt;tr&gt;&lt;td class=&quot;diff-marker&quot;&gt;&lt;/td&gt;&lt;td style=&quot;background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;&quot;&gt;&lt;div&gt;For standard exposure, empirical methods can relate dimensions and other parameters to results from furnace tests. Nonstandard exposure generally requires a more explicit thermal analysis followed by structural evaluation. Fleischmann and Buchanan describe both approaches and their different information requirements. A correlation derived from a standard test does not independently establish performance for an arbitrary natural fire.&amp;lt;ref name=&amp;quot;concreteinfi_FB_4-239&amp;quot; /&amp;gt;&lt;/div&gt;&lt;/td&gt;&lt;td class=&quot;diff-marker&quot;&gt;&lt;/td&gt;&lt;td style=&quot;background-color: #f8f9fa; color: #202122; font-size: 88%; border-style: solid; border-width: 1px 1px 1px 4px; border-radius: 0.33em; border-color: #eaecf0; vertical-align: top; white-space: pre-wrap;&quot;&gt;&lt;div&gt;For standard exposure, empirical methods can relate dimensions and other parameters to results from furnace tests. Nonstandard exposure generally requires a more explicit thermal analysis followed by structural evaluation. Fleischmann and Buchanan describe both approaches and their different information requirements. A correlation derived from a standard test does not independently establish performance for an arbitrary natural fire.&amp;lt;ref name=&amp;quot;concreteinfi_FB_4-239&amp;quot; /&amp;gt;&lt;/div&gt;&lt;/td&gt;&lt;/tr&gt;

&lt;!-- diff cache key firesb_pjbsiy42-wiki_:diff:1.41:old-3400:rev-3989:php=table --&gt;
&lt;/table&gt;</summary>
		<author><name>Linda</name></author>
	</entry>
	<entry>
		<id>https://fire-safety.academy/w/index.php?title=Prestressed_concrete_in_fire&amp;diff=3400&amp;oldid=prev</id>
		<title>Linda: New FSE wiki article: Prestressed concrete in fire (written by GPT-6)</title>
		<link rel="alternate" type="text/html" href="https://fire-safety.academy/w/index.php?title=Prestressed_concrete_in_fire&amp;diff=3400&amp;oldid=prev"/>
		<updated>2026-11-07T21:24:29Z</updated>

		<summary type="html">&lt;p&gt;New FSE wiki article: Prestressed concrete in fire (written by GPT-6)&lt;/p&gt;
&lt;p&gt;&lt;b&gt;New page&lt;/b&gt;&lt;/p&gt;&lt;div&gt;&amp;#039;&amp;#039;&amp;#039;Prestressed [[Concrete in fire|concrete in fire]]&amp;#039;&amp;#039;&amp;#039; concerns the response of concrete members containing deliberately tensioned steel when they are heated by a fire. Their resistance depends on the temperatures and properties of both concrete and steel, together with the force initially introduced by prestressing. The SFPE Handbook treats reinforcement temperature and structural continuity as parts of the member assessment.&amp;lt;ref name=&amp;quot;FB-pre&amp;quot;&amp;gt;Fleischmann and Buchanan (2002), pp. 4-239–4-246.&amp;lt;/ref&amp;gt;&amp;lt;ref name=&amp;quot;NFPA-§19.2,pp.19-53-19-54&amp;quot;&amp;gt;Cote et al. (2008), §19.2, pp. 19-53–19-54.&amp;lt;/ref&amp;gt;&lt;br /&gt;
&lt;br /&gt;
Concrete cover delays heating of embedded steel, but it does not prevent heating indefinitely. [[Spalling]] can remove that protection and change the exposed geometry. The NFPA Fire Protection Handbook gives particular attention to the initial stress and temperature sensitivity of prestressing steel. Those characteristics distinguish its response from an otherwise similar member with ordinary reinforcement.&amp;lt;ref name=&amp;quot;NFPA-§19.2,pp.19-53-19-54&amp;quot; /&amp;gt;&lt;br /&gt;
&lt;br /&gt;
The assessment therefore follows heat transfer, changing material properties and the complete resisting system. A classification as [[Fire-resistive construction|fire-resistive construction]] does not replace these member-specific conditions. Inspection after a fire also has to consider losses that remain after cooling.&amp;lt;ref name=&amp;quot;NFPA-§19.4,pp.19-65,19-73&amp;quot;&amp;gt;Cote et al. (2008), §19.4, pp. 19-65, 19-73.&amp;lt;/ref&amp;gt;&lt;br /&gt;
&lt;br /&gt;
== Prestress, heating and the resisting system ==&lt;br /&gt;
&lt;br /&gt;
Prestressing introduces forces before the member carries its full service loading. The NFPA handbook explains that the steel therefore begins fire exposure under substantial initial stress. Heating changes its strength, stiffness and time-dependent deformation. These effects can reduce the prestressing force and the capacity of the complete member.&amp;lt;ref name=&amp;quot;NFPA-§19.2,p.19-53&amp;quot;&amp;gt;Cote et al. (2008), §19.2, p. 19-53.&amp;lt;/ref&amp;gt;&lt;br /&gt;
&lt;br /&gt;
The distinction from ordinary reinforced concrete is not simply a different concrete strength. The function and type of steel matter, as do the initial force and its transfer into the concrete. [[Strength reduction at elevated temperatures]] must therefore be represented for the actual tendon material. A relationship for ordinary hot-rolled reinforcement does not establish every prestressing-steel response.&amp;lt;ref name=&amp;quot;NFPA-§19.2,pp.19-53-19-54&amp;quot; /&amp;gt;&lt;br /&gt;
&lt;br /&gt;
Concrete in fire develops temperature gradients because heat enters through exposed surfaces. A tendon close to a heated face can become hotter than reinforcement farther inside. Loss of cover changes that relationship. The SFPE analysis relates reinforcement temperature to the temperature distribution at its depth, while retaining the exposure geometry and member dimensions.&amp;lt;ref name=&amp;quot;FB-pre&amp;quot; /&amp;gt;&lt;br /&gt;
&lt;br /&gt;
The [[Load combination for fire|load combination for fire]] defines the external actions to be resisted. Prestress, thermal expansion and restraint then affect how these actions are carried. The NFPA handbook describes upward movement caused by differential thermal expansion as one possible prestressed-member response. The direction of visible movement alone therefore does not establish an uncomplicated bending mechanism.&amp;lt;ref name=&amp;quot;NFPA-§19.2,pp.19-53-19-54&amp;quot; /&amp;gt;&amp;lt;ref name=&amp;quot;NFPA-§19.5,pp.19-93-19-94&amp;quot;&amp;gt;Cote et al. (2008), §19.5, pp. 19-93–19-94.&amp;lt;/ref&amp;gt;&lt;br /&gt;
&lt;br /&gt;
== Cover, connections and the condition after cooling ==&lt;br /&gt;
&lt;br /&gt;
Cover is part of the thermal protection around the steel. Its effectiveness depends on remaining in place and on the distance from the exposed face to the tendon. The NFPA handbook notes that spalling can expose prestressing steel directly. The member then has both a changed cross-section and a changed heating boundary.&amp;lt;ref name=&amp;quot;NFPA-§19.2,pp.19-53-19-54&amp;quot; /&amp;gt;&lt;br /&gt;
&lt;br /&gt;
A floor or roof is also a system of members and supports. Precast elements, bearings and connections have different dependencies from a continuous cast-in-place arrangement. The handbook&amp;#039;s firefighting discussion explains that roof loss can remove restraint from heavy wall panels. The structural consequences can extend beyond the heated concrete element.&amp;lt;ref name=&amp;quot;NFPA-§12.8,p.12-136&amp;quot;&amp;gt;Cote et al. (2008), §12.8, p. 12-136.&amp;lt;/ref&amp;gt;&lt;br /&gt;
&lt;br /&gt;
Post-tensioned construction contains tendons whose continuity is part of the resisting mechanism. The handbook identifies damage to those tendons as a particular concern during fire operations and subsequent work. Appearance alone may not distinguish the system from ordinary reinforced concrete. Construction information therefore affects the interpretation of observed damage.&amp;lt;ref name=&amp;quot;NFPA-§12.8,p.12-136&amp;quot; /&amp;gt;&lt;br /&gt;
&lt;br /&gt;
[[Post-fire structural assessment]] examines residual force, deformation and material condition. Cooling does not automatically restore the initial prestress or every steel property. The handbook distinguishes prestressing steel from ordinary reinforcement in this respect. Its material discussion supports a separate investigation of the actual member rather than a general assumption of recovery.&amp;lt;ref name=&amp;quot;NFPA-§19.2,p.19-54&amp;quot;&amp;gt;Cote et al. (2008), §19.2, p. 19-54.&amp;lt;/ref&amp;gt;&amp;lt;ref name=&amp;quot;NFPA-§19.4,p.19-73&amp;quot;&amp;gt;Cote et al. (2008), §19.4, p. 19-73.&amp;lt;/ref&amp;gt;&lt;br /&gt;
&lt;br /&gt;
The same distinction affects interpretation of tests. A fire test represents a specified member, loading and restraint. A calculation represents its stated thermal and structural assumptions. Neither provides a transferable rating for every tendon arrangement, cover depth or support condition. The evidence remains attached to the complete configuration being assessed.&amp;lt;ref name=&amp;quot;FB-pre&amp;quot; /&amp;gt;&lt;br /&gt;
&lt;br /&gt;
== Heat penetration and material properties ==&lt;br /&gt;
&lt;br /&gt;
Heat entering the exposed surface moves through solid concrete mainly by conduction. Thermal conductivity describes how readily a temperature difference drives that transfer. Density and specific heat describe the energy stored as the material warms. Together, these quantities determine how rapidly a temperature disturbance spreads into the section.&amp;lt;ref name=&amp;quot;concreteinfi_FB_4-242&amp;quot;&amp;gt;Fleischmann and Buchanan (2002), p. 4-242.&amp;lt;/ref&amp;gt;&amp;lt;ref name=&amp;quot;concreteinfi_VR_5.2&amp;quot;&amp;gt;Van Rossum (2027), §5.2.&amp;lt;/ref&amp;gt;&lt;br /&gt;
&lt;br /&gt;
The exposed surface and the interior therefore need not reach the same temperature. During early heating, a substantial temperature gradient can exist through a thick section. The cooler interior is one reason a concrete member may continue functioning while its surface becomes very hot. A single furnace temperature does not represent the temperature of every reinforcement bar.&amp;lt;ref name=&amp;quot;concreteinfi_FB_4-239&amp;quot;&amp;gt;Fleischmann and Buchanan (2002), p. 4-239.&amp;lt;/ref&amp;gt;&amp;lt;ref name=&amp;quot;concreteinfi_FB_4-242&amp;quot; /&amp;gt;&amp;lt;ref name=&amp;quot;concreteinfi_VR_5.2&amp;quot; /&amp;gt;&lt;br /&gt;
&lt;br /&gt;
Moisture changes the energy balance because evaporation consumes heat. Heating also changes the material itself, including its microstructure and relevant thermal properties. Van Rossum consequently treats calculations with constant properties as approximations. The diffusivity used at one stage of heating need not describe the entire fire exposure.&amp;lt;ref name=&amp;quot;concreteinfi_VR_5.2&amp;quot; /&amp;gt;&amp;lt;ref name=&amp;quot;concreteinfi_KH_1-157&amp;quot;&amp;gt;Kodur and Harmathy (2002), p. 1-157.&amp;lt;/ref&amp;gt;&lt;br /&gt;
&lt;br /&gt;
A steady calculation assumes that the temperature profile through the whole construction has already developed. That assumption can be unsuitable during the initial heating of a thick wall. A transient calculation instead follows the changing temperatures as energy enters and spreads through the material. This distinction affects both reinforcement temperature and heat transfer to the unexposed side.&amp;lt;ref name=&amp;quot;concreteinfi_VR_5.2&amp;quot; /&amp;gt;&amp;lt;ref name=&amp;quot;concreteinfi_FB_4-239&amp;quot; /&amp;gt;&lt;br /&gt;
&lt;br /&gt;
== A worked heat-penetration example ==&lt;br /&gt;
&lt;br /&gt;
Thermal diffusivity divides conductivity by the volumetric heat capacity, which is density multiplied by specific heat. For a sudden surface-temperature change, the square root of diffusivity multiplied by time gives a characteristic penetration depth. This depth describes a scale of temperature change, rather than a sharp front separating hot and cold concrete.&amp;lt;ref name=&amp;quot;concreteinfi_VR_5.2&amp;quot; /&amp;gt;&lt;br /&gt;
&lt;br /&gt;
&amp;lt;math display=&amp;quot;block&amp;quot;&amp;gt;\alpha=\frac{\lambda}{\rho c_p},\qquad d\approx\sqrt{\alpha t}&amp;lt;/math&amp;gt;&lt;br /&gt;
&lt;br /&gt;
{| class=&amp;quot;wikitable&amp;quot;&lt;br /&gt;
! Symbol !! Description !! Unit&lt;br /&gt;
|-&lt;br /&gt;
| &amp;lt;math&amp;gt;\alpha&amp;lt;/math&amp;gt; || Thermal diffusivity || m²/s&lt;br /&gt;
|-&lt;br /&gt;
| &amp;lt;math&amp;gt;\lambda&amp;lt;/math&amp;gt; || Thermal conductivity || W/(m·K)&lt;br /&gt;
|-&lt;br /&gt;
| &amp;lt;math&amp;gt;\rho&amp;lt;/math&amp;gt; || Density || kg/m³&lt;br /&gt;
|-&lt;br /&gt;
| &amp;lt;math&amp;gt;c_p&amp;lt;/math&amp;gt; || Specific heat || J/(kg·K)&lt;br /&gt;
|-&lt;br /&gt;
| &amp;lt;math&amp;gt;t&amp;lt;/math&amp;gt; || Heating duration || s&lt;br /&gt;
|-&lt;br /&gt;
| &amp;lt;math&amp;gt;d&amp;lt;/math&amp;gt; || Characteristic penetration depth || m&lt;br /&gt;
|}&lt;br /&gt;
&lt;br /&gt;
Van Rossum&amp;#039;s comparison of thick concrete and timber walls uses rounded concrete properties of 1.7 W/(m·K), 2,300 kg/m³ and 900 J/(kg·K). With these inputs, the calculated diffusivity is 8.21 × 10⁻⁷ m²/s. After 3,600 s, the characteristic depth is approximately 0.054 m, or 54 mm. The calculation reproduces the source example using unrounded intermediate values.&amp;lt;ref name=&amp;quot;concreteinfi_VR_5.2&amp;quot; /&amp;gt;&lt;br /&gt;
&lt;br /&gt;
That result does not mean that concrete outside a 54 mm layer remains exactly at its initial temperature. Nor does it identify a spalling depth, a damaged zone or the position of a failure boundary. The model has no mechanical failure criterion and uses fixed thermal properties. Its purpose is to explain the scale of transient heating in a thick material.&amp;lt;ref name=&amp;quot;concreteinfi_VR_5.2&amp;quot; /&amp;gt;&lt;br /&gt;
&lt;br /&gt;
A separate example in the same section considers a 200 mm concrete wall over the first 900 s. It uses a different stated diffusivity, 9.88 × 10⁻⁷ m²/s. The source&amp;#039;s approximate boundary between thermally thick and thin behaviour, twice the penetration depth, is then 60 mm. The 200 mm wall is thermally thick for that example, but this observation does not assign it a fire-resistance rating.&amp;lt;ref name=&amp;quot;concreteinfi_VR_5.2&amp;quot; /&amp;gt;&lt;br /&gt;
&lt;br /&gt;
== Spalling and loss of cover ==&lt;br /&gt;
&lt;br /&gt;
Spalling is the breaking away of concrete from the heated surface. Kodur and Harmathy distinguish early explosive loss from later loss associated with weakened material. The process matters because the section can lose both material and thermal protection. Reinforcement formerly enclosed by concrete may then receive more direct heating.&amp;lt;ref name=&amp;quot;concreteinfi_KH_1-163_1-164&amp;quot;&amp;gt;Kodur and Harmathy (2002), pp. 1-163–1-164.&amp;lt;/ref&amp;gt;&lt;br /&gt;
&lt;br /&gt;
One proposed mechanism involves moisture movement and pressure within the pores. Heating drives moisture towards cooler regions, where a relatively saturated zone can impede further transport. Pressure can rise if vapour cannot escape readily. The handbook also discusses explanations based on thermal stresses and fracture, so pore pressure is not the sole mechanism considered.&amp;lt;ref name=&amp;quot;concreteinfi_KH_1-163&amp;quot;&amp;gt;Kodur and Harmathy (2002), p. 1-163.&amp;lt;/ref&amp;gt;&lt;br /&gt;
&lt;br /&gt;
The source illustrates the pressure mechanism using approximately 8 MPa vapour pressure at 300 °C and approximately 5 MPa tensile strength for high-strength concrete. This comparison demonstrates how internal pressure can exceed a resisting tensile stress; it is an explanatory example, not a universal pressure-temperature failure rule. Actual spalling also depends on permeability, moisture, loading and the heating conditions.&amp;lt;ref name=&amp;quot;concreteinfi_KH_1-163_1-164&amp;quot; /&amp;gt;&lt;br /&gt;
&lt;br /&gt;
High compressive strength at room temperature does not by itself prevent spalling. Dense, low-permeability concrete can restrict moisture escape during rapid heating. Once surface material is lost, deeper concrete and reinforcement heat more rapidly. A model that retains the original section throughout the exposure cannot automatically represent that change.&amp;lt;ref name=&amp;quot;concreteinfi_KH_1-163_1-164&amp;quot; /&amp;gt;&lt;br /&gt;
&lt;br /&gt;
Thermal stress offers a different way for cracking to develop. The heated surface tends to expand while cooler material restricts that movement. Kodur and Harmathy discuss fracture-based explanations in which these stresses contribute to surface loss. An analysis based only on vapour pressure therefore addresses one proposed contribution, rather than demonstrating that other mechanisms are absent.&amp;lt;ref name=&amp;quot;concreteinfi_KH_1-163&amp;quot; /&amp;gt;&lt;br /&gt;
&lt;br /&gt;
The distinction between tensile and compressive behaviour is also relevant. The pressure example compares internal pressure with tensile resistance, whereas the familiar concrete grade describes compressive strength; these are different material quantities. Increasing the specified compressive strength cannot by itself resolve a cracking mechanism involving internal pressure, restrained expansion and tensile fracture.&amp;lt;ref name=&amp;quot;concreteinfi_KH_1-163_1-164&amp;quot; /&amp;gt;&lt;br /&gt;
&lt;br /&gt;
== Reinforcement and load-carrying capacity ==&lt;br /&gt;
&lt;br /&gt;
Strength reduction at elevated temperatures affects both the concrete and the embedded steel. Fleischmann and Buchanan distinguish hot-rolled reinforcement from cold-drawn prestressing steel and high-strength alloy steel, and their strength-temperature relationships differ, reflecting the materials and mechanical properties considered. A single generic steel curve cannot represent every reinforced or prestressed member.&amp;lt;ref name=&amp;quot;concreteinfi_FB_4-239_4-240&amp;quot;&amp;gt;Fleischmann and Buchanan (2002), pp. 4-239–4-240.&amp;lt;/ref&amp;gt;&lt;br /&gt;
&lt;br /&gt;
Concrete strength also depends on aggregate and on the conditions of the material test. The handbook compares specimens heated under load with specimens heated before being loaded to failure, and these procedures can produce different measured strengths at the same temperature. Material data therefore need an accompanying description of the loading and heating history.&amp;lt;ref name=&amp;quot;concreteinfi_FB_4-240_4-241&amp;quot;&amp;gt;Fleischmann and Buchanan (2002), pp. 4-240–4-241.&amp;lt;/ref&amp;gt;&lt;br /&gt;
&lt;br /&gt;
The modulus of elasticity describes stiffness, or resistance to elastic deformation, and it can decrease substantially during heating even when part of the compressive strength remains. Consequently, a strength calculation and a deformation calculation address different effects. Thermal expansion adds another source of deformation and can alter the forces arising in restrained construction.&amp;lt;ref name=&amp;quot;concreteinfi_FB_4-240_4-241&amp;quot; /&amp;gt;&lt;br /&gt;
&lt;br /&gt;
In a simplified thermal analysis, the reinforcement temperature may be approximated by the concrete temperature at the bar centre. This connects the heat-transfer calculation to the subsequent structural calculation. The cover depth, exposed faces and heating duration then affect the steel properties used in that analysis. The approximation belongs to the stated modelling approach, rather than every possible member configuration.&amp;lt;ref name=&amp;quot;concreteinfi_FB_4-242&amp;quot; /&amp;gt;&lt;br /&gt;
&lt;br /&gt;
The load present during heating affects how a property curve is established. In the concrete results discussed by Fleischmann and Buchanan, some specimens carried 40% of their compressive strength while being heated. They were then loaded to failure at the temperature of interest. That procedure describes strength while hot, rather than a measurement of residual strength after cooling.&amp;lt;ref name=&amp;quot;concreteinfi_FB_4-240&amp;quot;&amp;gt;Fleischmann and Buchanan (2002), p. 4-240.&amp;lt;/ref&amp;gt;&lt;br /&gt;
&lt;br /&gt;
A temperature-dependent property curve consequently carries more information than its axes alone, and its concrete type, initial condition and testing sequence affect what the result represents. A curve measured for one aggregate and load history cannot be assumed to describe another without supporting evidence. This is separate from uncertainty in the furnace temperature or the calculated temperature within the member.&amp;lt;ref name=&amp;quot;concreteinfi_FB_4-240_4-241&amp;quot; /&amp;gt;&lt;br /&gt;
&lt;br /&gt;
== Beams, slabs and structural continuity ==&lt;br /&gt;
&lt;br /&gt;
A simply supported slab provides a useful starting model: its ends permit expansion and rotation under the idealised support conditions described by Fleischmann and Buchanan. As reinforcement heats and weakens, the section&amp;#039;s resistance to bending decreases. Structural failure is assessed by comparing that remaining resistance with the bending demand from the applied load.&amp;lt;ref name=&amp;quot;concreteinfi_FB_4-245&amp;quot;&amp;gt;Fleischmann and Buchanan (2002), p. 4-245.&amp;lt;/ref&amp;gt;&lt;br /&gt;
&lt;br /&gt;
Concrete near the compression face may remain cooler than reinforcement near the fire-exposed underside. The structural calculation therefore uses the temperature distribution, rather than applying one reduction to the entire section. If part of the compression zone becomes sufficiently hot, the source method reduces its contribution. That step depends on the chosen material model and calculation procedure.&amp;lt;ref name=&amp;quot;concreteinfi_FB_4-245&amp;quot; /&amp;gt;&lt;br /&gt;
&lt;br /&gt;
A continuous member behaves differently because it can redistribute bending moments between the span and its supports. Redistribution can extend endurance, but the remaining sections must still resist the transferred demand. Fleischmann and Buchanan describe failure through the formation of a mechanism involving several yielding regions. Continuity is therefore a structural condition, not an automatic allowance added to a rating.&amp;lt;ref name=&amp;quot;concreteinfi_FB_4-246&amp;quot;&amp;gt;Fleischmann and Buchanan (2002), p. 4-246.&amp;lt;/ref&amp;gt;&lt;br /&gt;
&lt;br /&gt;
Structural fire engineering combines this structural response with the preceding fire and thermal calculations. The assessment depends on loads, geometry, reinforcement and support conditions as well as temperature. More specialised structural behaviour is addressed in the related topic Tensile membrane action. The heat-penetration example above does not calculate any redistribution or membrane resistance.&amp;lt;ref name=&amp;quot;concreteinfi_FB_4-239&amp;quot; /&amp;gt;&amp;lt;ref name=&amp;quot;concreteinfi_FB_4-245_4-246&amp;quot;&amp;gt;Fleischmann and Buchanan (2002), pp. 4-245–4-246.&amp;lt;/ref&amp;gt;&lt;br /&gt;
&lt;br /&gt;
== Testing and fire-resistance assessment ==&lt;br /&gt;
&lt;br /&gt;
Fire resistance is evaluated against specified functions under a defined exposure. A separating concrete floor may need to support loads and limit heat transfer to the space above. A column has a different structural role and exposure arrangement. The required endpoints follow the assembly and assessment method, rather than the material name alone.&amp;lt;ref name=&amp;quot;concreteinfi_FB_4-239&amp;quot; /&amp;gt;&amp;lt;ref name=&amp;quot;concreteinfi_FB_4-242&amp;quot; /&amp;gt;&lt;br /&gt;
&lt;br /&gt;
For standard exposure, empirical methods can relate dimensions and other parameters to results from furnace tests. Nonstandard exposure generally requires a more explicit thermal analysis followed by structural evaluation. Fleischmann and Buchanan describe both approaches and their different information requirements. A correlation derived from a standard test does not independently establish performance for an arbitrary natural fire.&amp;lt;ref name=&amp;quot;concreteinfi_FB_4-239&amp;quot; /&amp;gt;&lt;br /&gt;
&lt;br /&gt;
New Zealand&amp;#039;s C/VM2, second edition of 2025, defines a fire resistance rating using three durations, and their order is structural adequacy, integrity and insulation. The definition permits standard testing or a specified calculation method verified against standard fire-resistance tests. This is the terminology of that New Zealand document, rather than a universal notation for every jurisdiction.&amp;lt;ref name=&amp;quot;concreteinfi_CVM_64&amp;quot;&amp;gt;Ministry of Business, Innovation and Employment (2025), p. 64.&amp;lt;/ref&amp;gt;&lt;br /&gt;
&lt;br /&gt;
== See also ==&lt;br /&gt;
&lt;br /&gt;
&lt;br /&gt;
&lt;br /&gt;
== Notes ==&lt;br /&gt;
&lt;br /&gt;
&amp;lt;references /&amp;gt;&lt;br /&gt;
&lt;br /&gt;
== References ==&lt;br /&gt;
&lt;br /&gt;
* Cote, A. E., Grant, C. C., Hall, J. R., Jr., &amp;amp; Solomon, R. E. (Eds.). (2008). &amp;#039;&amp;#039;Fire protection handbook&amp;#039;&amp;#039; (20th ed.). National Fire Protection Association.&lt;br /&gt;
* Fleischmann, C., &amp;amp; Buchanan, A. (2002). Analytical methods for determining fire resistance of concrete members. In P. J. DiNenno (Ed.), &amp;#039;&amp;#039;SFPE handbook of fire protection engineering&amp;#039;&amp;#039; (3rd ed., pp. 4-239–4-256). National Fire Protection Association.&lt;br /&gt;
* Kodur, V. K. R., &amp;amp; Harmathy, T. Z. (2002). Properties of building materials. In P. J. DiNenno (Ed.), &amp;#039;&amp;#039;SFPE handbook of fire protection engineering&amp;#039;&amp;#039; (3rd ed., pp. 1-155–1-181). National Fire Protection Association.&lt;br /&gt;
* Ministry of Business, Innovation and Employment. (2025). &amp;#039;&amp;#039;C protection from fire: Verification method C/VM2&amp;#039;&amp;#039; (2nd ed.).&lt;br /&gt;
* Van Rossum, E. (2027). &amp;#039;&amp;#039;Introduction to Fire Safety Engineering&amp;#039;&amp;#039;. Fire Safety Academy.&lt;br /&gt;
&lt;br /&gt;
[[Category:Structural Fire Engineering]]&lt;/div&gt;</summary>
		<author><name>Linda</name></author>
	</entry>
</feed>